Skip links

Refractory Materials FAQ - CH Refractories

One complete reference for buyers of refractory materials: company and ordering questions, steel and ladle lining, cement kilns, glass kilns and AZS, nonferrous smelting, power and petrochemical service, industrial furnaces, and engineering, installation and troubleshooting. Jump to any section below, or expand a question for the full answer.

FAQ contents - jump to any section
  1. About CH Refractories, Ordering and Service (40)
  2. Steel Industry, Ladle and Continuous Casting Refractory (55)
  3. Cement Kiln Refractory: Zones, Materials, Coating and Service (46)
  4. Glass Kiln Refractory and AZS (42)
  5. Nonferrous Casting Refractory: Copper, Nickel, Zinc and Lead Smelting (35)
  6. Power and Petrochemical Refractory (41)
  7. Industrial Furnace Refractory (37)
  8. Refractory Lining Engineering, Installation and Troubleshooting (48)

About CH Refractories, Ordering and Service

Questions: 40

Questions in this section
  1. About CH Refractories (10)
  2. Products & Industries (3)
  3. Ordering, Logistics & Payment (20)
  4. Services & Market (7)

About CH Refractories

Q1. What is CH Refractories?

CH Refractories is the export brand of Zhengzhou Caihua Kiln Masonry Installation Co., Ltd., founded in 1984 in Xinmi City, Henan Province, China. It is a refractory manufacturer and turnkey refractory engineering solution provider for high-temperature kilns, with more than 40 years of industry experience, 1,281 employees, annual production capacity above 50,000 tons, and products spanning shaped bricks, unshaped materials, functional refractories and ceramic fibre.

Q2. Where is your factory and how do I reach it?

The factory is in Yuanzhuang Town Industrial Park, Xinmi City, Henan Province, China, about 50 km and 50 minutes by car from Zhengzhou Xinzheng International Airport, and about 40 km from Zhengzhou East High-Speed Railway Station. The site sits on the Beijing-Guangzhou and Longhai rail corridors, with a container trailer distance of roughly 600 to 800 km to the northern ports of Qingdao, Tianjin and Lianyungang.

Q3. What is your annual production capacity and what equipment do you run?

Annual capacity exceeds 50,000 tons. The plant operates a 111-metre high-temperature tunnel kiln, two 180-metre and one 120-metre tunnel kilns, a shuttle kiln, a microcomputer-controlled automatic batching system, and presses from 60 t to 2,500 t, including 2 units of 1,000 t, 4 of 630 t, 14 of 400 t, 22 of 315 t, 2 of 160 t and 8 of 60 t, together with a 2,500 t LAEIS press and a 1,000 t electric screw press.

Q4. Which quality standards and certifications do you follow?

Production runs under the ISO 9001 quality management system, and every batch is inspected and fully traceable. Product physical and chemical indicators are designed to ASTM, GB/T and ISO refractory standards. Certification coverage includes ISO 9001, foreign trade operator registration, Zhengzhou-level Top 100 Key Private Enterprise, Grade A tax credit rating and provincial high-quality product title. The company is also an active member of CARI, the China Association of Refractories Industry.

Q5. What design and engineering services do you provide?

The engineering team works with Solidworks 3D modelling and 3D CFD fluid-thermal simulation. Deliverables include 3D refractory lining design, custom special-shaped brick and precast block engineering, thermal stress and mechanical load analysis, installation brick-layout drawings with per-brick BOM lists, and on-site masonry guidance. A typical Steelworks ladle or blast furnace tuyere package runs 1 to 2 weeks of design and simulation.

Q6. What is the 100% factory pre-assembly process?

For composite assemblies such as blast furnace tuyere zones, finished bricks are physically pre-assembled 1:1 on factory platforms strictly to the drawings. Every brick's dimensional accuracy and joint requirement is verified before numbering and shipment, so there are zero fit problems on site. The same process has delivered extreme construction precision on projects such as the Jiuquan Steel 1,080 m3 hot blast stove.

Q7. Do you provide on-site installation supervision?

Yes. Senior refractory engineers with more than ten years of practical experience are dispatched for resident or travelling installation supervision, with experienced masons assigned to critical areas for dimensional verification and expansion joint checks. The customer's own team can be trained over 3 to 5 days covering refractory installation, hot repair technique and safety procedures.

Q8. What is your project workflow from design to hot repair?

Six steps: engineering design with CFD simulation and Solidworks modelling; precision manufacturing with full-batch ISO 9001 inspection; on-site installation under senior engineers; furnace drying and commissioning with hot commissioning, baseline performance measurement and operator training; after-sales operation and maintenance with resident inspection and life assessment; and hot repair support with rapid gunning mix supply and 48-hour spare parts response.

Q9. How do you differ from a pure product supplier?

The company operates as a turnkey engineering partner rather than a brick seller: 3D CFD simulation to fix airflow before the furnace is built, a Solidworks solid assembly library for ladles and composite combined bricks, and senior engineers on site to land the drawing. The Jiuquan Steel 1,080 m3 hot blast stove, delivered with a service life guarantee of more than 15 years, is the reference project behind this claim.

Q10. How do you support low-carbon and green steelmaking?

Working with global green steel pioneers, the company develops refractory formulations for hydrogen corrosion and optimised for low carbon: high-purity magnesia-chrome bricks specially developed for hydrogen-based direct reduced iron, oxidation-resistant enhanced MgO-C bricks adapted to high-oxygen EAFs, kiln thermal modelling designed for energy efficiency limits, and advanced hot repair solutions that cut refractory solid waste and extend campaign life.

Products & Industries

Q11. How broad is your product range?

125 core products across 13 high-temperature equipment categories: blast furnace, hot blast stove, electric arc furnace, ladle, tundish, continuous casting machine, secondary refining furnace, induction furnace, cement rotary kiln, glass melting furnace, nonferrous metal smelting furnace, power and petrochemical boiler, industrial heating furnace, and refractory raw materials.

Q12. Which industries do you serve?

Six core fields: steel, cement, glass, nonferrous metals, power and petrochemical, and industrial kilns. Within steel the complete production route is covered, from blast furnace through converter and EAF, ladle and tundish, to continuous casting, together with the LF, RH, CAS-OB and VD secondary refining systems.

Q13. Which countries have you supplied?

More than 50 countries and regions. Products and engineering services broadly cover Southeast Asia, the Middle East, Europe, Africa and the Americas, supported by local agents in several core heavy-industry markets.

Ordering, Logistics & Payment

Q14. What is the typical delivery lead time?

Standard brick production takes about 2 to 3 weeks. Custom special-shaped bricks take about 2 to 4 weeks depending on mould and formulation complexity. Solidworks 3D thermal modelling and 3D CFD fluid simulation design take about 1 to 2 weeks. The specific delivery date is confirmed against the production scheduling of each order.

Q15. What shipping terms do you support?

All INCOTERMS are supported, from basic FOB through CFR and CIF, with DAP and DDP available on request, and global shipment tracking. Export goods are packed in export-grade reinforced fumigation-free wooden cases with moisture-proof film lining for safe, damage-free long-distance sea and land transport.

Q16. Which ports and shipping routes do you use?

The core export positions are the super deep-water ports of northern China: Qingdao and Tianjin, plus Lianyungang in Jiangsu, with a container trailer distance of about 600 to 800 km. For special routes or very large bulk vessel orders, sailings are also arranged from Shanghai Port and Ningbo-Zhoushan Port.

Q17. How long does ocean shipping typically take?

Main route benchmarks: Qingdao to Rotterdam 28 to 32 days, to Hamburg 30 to 34 days, direct to Dubai (Jebel Ali) 18 to 22 days, Lianyungang to Mumbai 15 to 18 days, across the Pacific to Los Angeles 16 to 20 days, and to Santos in Brazil 35 to 40 days. Actual transit varies with schedule and routing.

Q18. How much can you load per container?

A standard 20-foot general purpose container can hold about 25 tons of high-density monolithic material in bags, or about 18 tons of heavy-duty shaped refractory bricks on wooden pallets. A 40-foot high cube container carries about 28 tons. For orders of thousands or tens of thousands of tons, ocean-going bulk carriers are chartered, and the China-Europe Railway Express is also available for direct Central Asian and European delivery.

Q19. What packaging standards do you follow?

Shaped bricks are stacked on solid wood pallets with anti-impact corner protectors, covered with waterproof shrink film and strapped with high-strength steel strips or PET plastic steel strapping, at 1 to 1.5 tons per pallet. Monolithic bulk material is packed in 25 kg or 50 kg three-layer moisture-proof kraft paper or woven bags. Precast blocks and AZS blocks ship in closed fumigation-free wooden cases lined with high-density shock-absorbing foam.

Q20. Do wooden pallets meet fumigation requirements?

Yes. All solid wooden pallets, dunnage and sealed wooden cases strictly implement the international ISPM 15 standard, undergo thorough heat treatment or methyl bromide fumigation, and are clearly stamped with the IPPC mark on the wood surface, so clearance in strict quarantine markets such as the United States, the European Union, Australia and India is straightforward.

Q21. What documents accompany each shipment?

The standard shipping document package includes a stamped commercial invoice, detailed packing list, chamber of commerce or customs Certificate of Origin, detailed physical and chemical quality certificate, Material Safety Data Sheet, marine insurance certificate, original bill of lading or air waybill, and the international fumigation certificate required for wooden packaging.

Q22. What payment terms do you accept?

The conventional international standard is T/T, with 30% deposit on order confirmation and the 70% balance settled before shipment against a copy of the bill of lading. For senior strategic customers, irrevocable sight L/C at 100%, 30, 60 or 90-day open account sales subject to strict credit approval, and D/P are all available.

Q23. How long is a quotation valid, and what does it include?

The official system quotation for standard finished products is locked for 30 days. When core market resources such as high-grade fused magnesia, premium bauxite or natural flake graphite tighten or move sharply, the validity is dynamically shortened to 15 days to protect both parties. The EXW price covers product value and export-grade reinforced packaging; inland haulage, customs declaration, ocean freight, marine cargo insurance and destination clearance are itemised separately.

Q24. What is your sample policy?

For standard conventional shaped blocks and bulk powder, a complete set of small samples is sent free of charge, usually 5 kg or less, with only the international express postage for the buyer to cover. For proprietary custom formulations, a special mould-opening R&D fee may be charged, but it is fully offset against the bulk production order that follows.

Q25. Will you sign a non-disclosure agreement before technical exchange?

Yes. Before any in-depth technical exchange, core drawing release or detailed solution quotation, the company is willing to sign a bilateral non-disclosure agreement to protect both parties' technical and commercial secrets. The customer's own bilingual NDA template can be used, or the company's standard template is supplied.

Q26. Can we arrange a factory audit?

Very welcome. The company accepts and actively cooperates with customers' in-depth factory audits; please make an appointment at least 7 days in advance. The audit process usually includes a panoramic factory tour, an in-depth technical seminar, laboratory practical demonstration, and an on-site display of 3D engineering R&D capability.

Q27. Which countries require special export certifications?

Global trade barriers require crossing high-threshold mandatory access certification: exports to India of core industrial products are firmly controlled by BIS, Saudi customs clearance mandatorily requires SASO inspection and release, former Soviet CIS countries require Russia EAC Customs Union compliance endorsement, the European Union mandates CE environmental and safety testing, Brazil requires INMETRO strict access, and Indonesia and Malaysia apply SNI and MS MARK respectively.

Q28. Can we have third-party witnessed testing?

Completely open and welcome, and the company encourages third-party inspection. It maintains full cooperation with international inspection and certification institutions including SGS, Bureau Veritas, CCIC and German TUV Rheinland. Institutions need to be scheduled 5 to 7 days in advance, and their experts enter the factory laboratory to witness sampling, specimen preparation and destructive pressing.

Q29. How is each batch quality controlled?

Every batch goes through strict multi-dimensional laboratory inspection: XRF spectral analysis of the full chemical composition, bulk density and apparent porosity measurement, heavy-duty press measurement of cold crushing strength and modulus of rupture, and verification of refractoriness, refractoriness under load, thermal shock cracking cycles and high-temperature static and dynamic slag corrosion in high-temperature electric furnaces. Automated precision scanning is combined with strict manual selection, and each batch carries a traceable ISO 9001 anti-counterfeiting code.

Q30. How do you handle an emergency or a quality claim?

For extremely critical quality complaints or catastrophic on-site events such as sudden furnace penetration, the company commits to sound the alarm at the first time and respond fully within 24 hours through the director-level dedicated line and email. The technical team provides rescue and repair prescription drawings within 48 hours, and emergency spare parts needing air freight are cleared and shipped within 48 hours.

Q31. What warranty and post-commissioning service do you provide?

The company sells long-term protection. Written commitments are given for a campaign life of more than 15 years on hot blast stove core linings and more than 8 years in nonferrous smelting environments. Remote expert diagnosis is available 7x24 hours covering multiple languages, engineers train the operating team on site for 3 to 5 days, and on-site inspection and evaluation are provided during every planned overhaul.

Q32. Do you support long-term framework agreements?

Yes. Deep medium- and long-term annual or multi-year strategic framework agreements are welcome with global group buyers. These lock down minimum volume commitments, an equitable commodity price linkage mechanism, strict acceptance quality standards, safety stock with priority shipment allocation, and flexible large credit terms.

Q33. How do I contact you?

Official hotline +86-371-69987777, mobile and WhatsApp +86 137 2142 5142, business email info@chrefractorygroup.com. Working hours are Beijing time Monday to Friday, 08:00 to 21:00. A senior metallurgical and refractory team proficient in Chinese, English and Russian is on duty, with the first customised technical response promised within 24 hours of receiving the working condition enquiry.

Services & Market

Q34. Do you attend international exhibitions?

Actively. As an active core member of CARI, the company frequently appears at the China Association of Refractories Industry annual meeting, which focuses on green manufacturing, low-carbon transformation and high-end refractories, and at international events such as METEC in Germany.

Q35. What is the global refractory market like in 2026?

Comprehensive research by multiple authoritative institutions, including Mordor Intelligence and Grand View Research, values the global market at approximately USD 39.1 billion in 2026, rising toward the USD 41 to 50 billion range on decarbonisation and infrastructure demand, with potential to reach USD 59 billion by 2031. Asia-Pacific holds roughly 73 to 75% of global demand.

Q36. Which industry consumes the most refractory material?

Steel manufacturing is the absolute consumption leader at about 62% of global consumption in 2025, with cement and building materials at 12 to 14%, nonferrous metal smelting at 8 to 10%, and glass and ceramics at 6 to 8%. The balance is petrochemical and waste incineration applications.

Q37. What are the structural trends shaping refractory demand?

Five trends: low-carbon metallurgy transition driving energy-saving, ultra-long-campaign materials; EAF capacity surge raising demand for oxidation-resistant MgO-C bricks and high-density monolithic linings; glass industry efficiency upgrades moving furnaces to AZS 41# bricks; cement plant cost optimisation, where alternative fuels raise alkali load and demand super alkali-resistant linings; and supply chain de-globalisation, pushing regional giants to localise spare parts sourcing.

Q38. How large is China's refractory industry?

China remains the core engine of global refractories. CARI data puts national total production capacity at about 25 million tons per year, supporting domestic steel groups producing over one billion tons. Leading Chinese suppliers have moved decisively into the global high-end market with AZS 41# fused blocks, ultra-high-purity MgO-C bricks and precision 3D composite bricks.

Q39. What does the 2030 industry goal look like?

CARI has set five-year sprint targets: manufacturing-side absolute carbon emissions down 30%; high-end special refractory products rising above 50% of total output; leading enterprises achieving fully unmanned digitalised factories from batching, forming to temperature measurement; capturing the drafting voice of international top refractory standards; and a substantial increase in share within core deep-water overseas markets such as Europe and America.

Q40. Which regional markets matter most for export?

The core base is the large Indian market, where infrastructure is on the eve of expansion. Southeast Asia is the basic plate through manufacturing transfer. Middle Eastern countries are building steel plants at scale. Africa is in the early industrialisation stage, Africa and Latin America continue to grow, and Europe and Russia are demanding higher-specification materials.

Steel Industry, Ladle and Continuous Casting Refractory

Questions: 55

Questions in this section
  1. Ladle Working Layer and Permanent Lining (6)
  2. Steel Making Vessels: BOF, EAF, LF, VD and RH (7)
  3. Tundish and Continuous Casting Flow Control (8)
  4. Slide Gate, Nozzles and Ladle Flow Control (6)
  5. Iron Runner, Taphole and Casting House (7)
  6. Gunning, Hot Repair and Unshaped Materials (6)
  7. Steel Plant Engineering and Service (7)
  8. Industry Knowledge for Refractory Buyers (8)

Ladle Working Layer and Permanent Lining

Q1. We reline on a hot-ladle turnaround. Which working layer form costs us the least site time?

Precast shapes, and the reason is where the work happens. Pre Cast Shapes For Working Layer (CH-GBY88, CH-GBY85) are cast, cured, fired and finished in the factory and shipped as single pieces for direct lifting, which saves on-site baking time and avoids construction hazards, with bulk density 3.00 to 3.05 g/cm3 and cold crushing strength 65 MPa minimum at 1550 °C. Castables For Working Layer (CH-GBJ88, CH-GBJ85, CH-GBJ80, CH-GBJ75) is the on-site alternative, and it still carries a curing, heating and drying cycle inside the shutdown window.

Q2. How do I choose between the four MgO-C brick grades for slag line, side wall and bottom?

Match carbon content to slag aggressiveness. CH-MT14A (MgO at least 76%, carbon at least 14%) is the premium high-carbon grade for the slag line, where slag resistance dominates. CH-MT14B (MgO at least 74%, carbon at least 14%) is the standard high-carbon grade for general ladle working lining. CH-MT10A (MgO at least 80%, carbon at least 10%) is the medium-carbon grade, balanced for wear plus oxidation resistance. CH-MT5A (MgO at least 85%, carbon at least 5%) is the lower-carbon grade for EAF working lining. Across the family apparent porosity is 6% maximum, bulk density 2.90 g/cm3 minimum and cold crushing strength 30 MPa minimum.

Q3. We make ultra-low-carbon steel and cannot accept carbon pick-up. What do I specify?

Specify a carbon-free working layer and keep carbon-bearing material out of the metal contact zone. Carbon Free Brick For Ladle Working Layer offers three grades: CH-LM85 (alumina at least 80%, magnesia 5 to 10%), CH-LM88 (alumina at least 85%, magnesia 3 to 6%) and CH-LM90 (alumina at least 90%, magnesia 3 to 6%), with apparent porosity 12% maximum, bulk density 2.95 to 3.10 g/cm3 and cold crushing strength 35 to 45 MPa. Behind it, Carbon Free And Environmental Friendly Dry Masses (CH-GK80, CH-GK70, CH-GK65) use an inorganic binder and sinter aid, so no toxic gas is released on installation and neither carbon nor hydrogen is added to the steel.

Q4. Which permanent lining family should I use: carbon-free dry mass, monolithic safety layer, or MgO-CaO dry mass?

Three families, and the choice is driven by how the permanent lining is installed and what chemistry the slag brings. Carbon-free dry masses CH-GK80 (MgO at least 80%), CH-GK70 (MgO at least 70%) and CH-GK65 (MgO 65% maximum, high calcium) give bulk density 1.8 to 2.2 g/cm3 and permanent linear change -3.0 to 0% after 1500 °C for 3 hours. Monolithic Castables For Ladle Safety Layer run CH-J-65 and CH-JZ70, CH-JZ75, CH-JZ80, CH-JZ85, cold crushing strength 45 to 60 MPa at 1500 °C. MgO / MgO-CaO / Forsterite Based Dry Masses add CH-GM70 to CH-GM88 and CH-TMG15.

Q5. Should the ladle bottom impact zone be brick, castable or a precast block?

Treat it as a separate engineering zone, because it takes the steel stream on every tap. Castables For Working Layer offers CH-GBJ88 and CH-GBJ85 for large and medium ladles and CH-GBJ80 and CH-GBJ75 for small and medium ladles and slag zone service, with cold crushing strength 60 to 65 MPa after 1550 °C for 3 hours. Pre Cast Shapes For Working Layer (CH-GBY88, CH-GBY85) deliver the same chemistry as a precast block, bulk density 3.00 to 3.05 g/cm3 and cold crushing strength 65 MPa minimum at 1550 °C, which removes site baking time. For clean steel, the low-carbon corundum-spinel brick is the specified choice in the bottom impact zone.

Q6. Which mortar do I use between ladle bricks, and why not a generic clay mortar?

Magnesia Mortar CH-DHN is the matching product: MgO-Al2O3 at least 90%, grain size 0 to 0.2 mm, hardening time 60 to 180 seconds and adhesive strength 1 MPa minimum. The short hardening window matters on a hot-side repair, and the chemistry matters more: it is chemically compatible with magnesia, magnesia-carbon, magnesia-chrome and forsterite brick, which is why it is specified for ladle and converter masonry joints. It is supplied as a single grade, and its full data sheet sits on the Magnesia Mortar product page.

Steel Making Vessels: BOF, EAF, LF, VD and RH

Q7. How should a BOF converter lining be zoned, and what life should I expect?

Zone it by function, because the bath, the trunnion and the slag line do completely different jobs. Modern converter working linings use high-quality MgO-C brick with grades matched to each part, and lining life can reach more than 1,500 to 4,000 heats. The safety lining behind it uses tar-bonded magnesia brick or fired magnesia brick, and the brick joints are filled with magnesia ramming mix. The slag line takes the most severe corrosion of anywhere in the vessel, so it normally runs premium grade MgO-C brick or resin-bonded dolomite brick.

Q8. For an EAF, which refractory goes where?

Four zones, four answers. The furnace wall working lining uses MgO-C brick. The slag line is strengthened with graphite content of 14% or more, or you move to MgO-CaO brick. The furnace bottom uses a magnesia-based dry ramming mix. The roof and electrode delta area use thermal-shock resistant high alumina or dolomite-based precast castables. For hydrogen-based DRI and high-oxygen smelting routes the package shifts again, to hydrogen-resistant high-purity magnesia-chrome brick, oxidation-resistant enhanced MgO-C brick, combined with gunning mix hot repair solutions.

Q9. What is the EAF bottom dry ramming mix made of, and why is it installed dry?

It is built on the principle of closest particle packing, with maximum particle size usually controlled at 6 to 8 mm, and is composed mainly of high-purity magnesia, a high iron-calcium sintering agent and special additives. It is installed completely dry, without water, and reaches maximum packing density through mechanical vibration. During the first heats after startup the surface sinters into a hard shell while the layer beneath stays a powdery buffer that absorbs thermal expansion stress and keeps steel from penetrating the bottom. Grades are CH-DLD85 (MgO 85% or higher), CH-DLD80 (MgO 80% or higher) and CH-DLD68 (MgO 68% or higher, CaO 18 to 25%).

Q10. EAF tapping hole: brick, filler, or both?

Both, and they are different products with different jobs. The block itself is Taphole Refractory Brick: CHDLC-14 (MgO 78% or higher, carbon 14% or higher) for high-carbon service and CHDLC-10 (MgO 82% or higher, carbon 10% or higher) for lower-carbon service, with apparent porosity 5% or less, bulk density 2.85 to 2.90 g/cm3 and cold crushing strength 50 MPa or higher. Between taps the gap is filled with Filler For EAF Tap Hole, a 2 to 6 mm granular material in CH-DCT90 (silica 90 to 95%), CH-DCT75 (silica 75% or higher, magnesia 10% or higher) or CH-DCT25 (magnesia 55% or higher).

Q11. What wears first in an LF ladle furnace, and how is it handled?

The electrode delta area, because arc radiation there is the most severe thermal load in the vessel. The sidewall slag line mostly uses MgO-C or MgO-CaO brick, the permanent lining is high alumina or corundum-based castable, and daily maintenance uses magnesia-based trowelling or gunning mix. The delta zone is handled with precast blocks: Pre Cast Shapes For Electrode Area Of Ladle Furnace LF covers CH-LFY80 (MgO+Al2O3 80% or higher), CH-LFY85, CH-LFY90 and CH-LFY92 (92% or higher with Cr2O3 2% or higher), cold crushing strength 40 MPa at 110 °C rising to 60 MPa at 1500 °C.

Q12. Why are VD covers and CAS-OB covers castable rather than brick?

Because they are lifted and lowered repeatedly while the vessel is hot, and because a large steel-fibre-reinforced cast cover cracks in a contained way instead of breaking. Splash Isolation Cover For VD Furnace gives CH-VD85 (MgO+Al2O3 85% or higher), CH-VD90 and CH-VD92 (92% or higher with Cr2O3 2% or higher), with cold crushing strength 40 MPa at 110 °C and 60 MPa at 1500 °C and permanent linear change ±0.5%. For CAS-OB the duty is split: Refractories For CAS-OB Refining uses CH-CAS88 (88% or higher) for the CAS cover and CH-OB90 (90% or higher) for the oxygen gun zone.

Q13. Which magnesia-chrome brick goes where in an RH degasser?

Match the grade to the duty, because the RH vacuum vessel and circulation tubes see extreme vacuum and high-speed circulating washing of molten steel. CH-MCr-D26 (MgO at least 53%, Cr2O3 at least 26%) is the fused re-bonded grade for circulation tubes and the bottom groove. CH-MCr-D20A and CH-MCr-B20A (fused semi re-bonded, MgO at least 50%, Cr2O3 at least 20%) cover dip tubes, bottom through and upper through. CH-MCr-B16A (direct-bonded, MgO at least 55%, Cr2O3 at least 16%) goes in the upper tube and hypo-working lining, and CH-MCr-Z8A (direct-bonded, MgO at least 65%, Cr2O3 at least 8%) in the secondary working lining.

Tundish and Continuous Casting Flow Control

Q14. How is a tundish lining built up, layer by layer?

Four layers with four separate jobs. The permanent lining is alumina-magnesia castable and acts as the safety and insulation layer. Between the permanent lining and the working lining sits a tundish board, calcium silicate or lightweight fibre insulation board, which reduces the temperature drop of the molten steel in the tundish. The working lining is magnesia-based or neutral dry vibrating material, installed with no water and cured by a light bake at about 200 °C. Flow control uses dams, weirs and flow stabiliser precast parts, and the surface is covered with an acidic or alkaline tundish covering agent for insulation and inclusion absorption.

Q15. Dry mass or dry vibrating material for the tundish working lining?

They suit different zones and different slag conditions. MgO / MgO-CaO / Forsterite Based Dry Masses cover the alkaline end: CH-GM70, CH-GM80, CH-GM85 and CH-GM88 on the magnesia and forsterite system, plus CH-TMG15 (MgO 70% or higher, CaO 10 to 20%). You pour the bag and vibrate with a template, bulk density 1.8 to 2.4 g/cm3, permanent linear change -3.0 to 0% after 1500 °C, and the residual lining strips easily afterwards. Where slag acidity swings, a near-neutral chemistry is steadier, which is the logic behind the neutral dry vibrating grade.

Q16. What is the correct tundish baking procedure?

It is a strict two-stage curve. First, gas baking burners run with a small flame for 90 to 120 minutes to remove all free water and raise the temperature smoothly. Then the burners switch to a large flame and the temperature is raised quickly to 1,000 to 1,100 °C, which sinters the working surface into a hard shell. From there the tundish goes into a holding state, waiting for steel tapping and casting. Shortening the small-flame stage is the classic mistake, because it is the stage that drives the free water out of the lining before steel ever touches it.

Q17. How do I select a monoblock stopper?

Start from the steel, because the nose takes the worst erosion and the body takes the rest. Four material systems are available: CH-SLT (Al2O3-C, alumina 50 to 72%) for general continuous casting service, CH-SMT (MgO-C, MgO 65% or higher) for demanding service, CH-SZT (ZrO2-C, ZrO2 50 to 60%) for the highest demand and CH-SMAT (Spinel-C, MgO 10% or higher) for special steel grades. Both argon-purging and non-purging mono-stoppers can be produced, and the nose can be Al2O3-C, MgO-C, Spinel-C or ZrO2-C. Bulk density 2.45 to 3.40 g/cm3, cold crushing strength 20 to 25 MPa, modulus of rupture 5 to 8 MPa, thermal shock resistance 5 cycles minimum.

Q18. Tundish upper nozzle or zirconia sizing nozzle: when do I need which?

The tundish upper nozzle is the flow-control channel embedded in the tundish well block, supplied as a matched body and bowl pair in three systems: CH-SK-L70 (Al2O3-C, alumina 40 to 72%), CH-SK-MA55 (MgO-C, MgO 10 to 65%) and CH-SK-X70 (ZrO2-C, ZrO2 50 to 60%), with bulk density 2.35 to 3.10 g/cm3, cold crushing strength 20 to 30 MPa, modulus of rupture 5 to 10 MPa and thermal shock resistance 5 cycles minimum. The zirconia sizing nozzle is the metering element for slab and bloom casting: a stabilised ultra-high-purity ZrO2 ring resists molten steel erosion, so the bore diameter hardly expands over casting sequences longer than ten hours.

Q19. Our submerged entry nozzles keep clogging with alumina inclusions. What can be done?

Three levers: material, installation type and gas. On material, CH-RZT is Al2O3-(ZrO2)-C(+SiC) based with alumina 45 to 55%, ZrO2 70% or higher in the slag line and C+SiC 11 to 28%, supplied in four parts, body, slag line, steel-tapping hole and bowl; CH-RS is fused silica based with alumina 65% or higher, MgO 99% or higher on the sliding plate surface and carbon 15% maximum. On installation, outside-stationed, quick-exchangeable, monolithic, thin-slab and anti-clogging nozzles are all available. On gas, argon blowing slits stop alumina inclusions adhering to the inner wall.

Q20. Pre-heated or pre-heat-free ladle shroud?

It depends on your casthouse capability and on the steel. Pre-heating required grades are CH-CZT-H (alumina 50% or higher, C+SiC 22% or higher) and CH-CLT-H (ZrO2 50% or higher, C+SiC 20% or higher). Pre-heat-free grades are CH-CZT (alumina 60% or higher, C+SiC 26% or higher) and CH-CLT (alumina 45% or higher, C+SiC 20% or higher). A non-protective fired, pre-heat-free shroud can also be supplied, and under a special firing process the shroud develops a de-carbonised layer with micropores, giving better insulation, a favourable temperature gradient and better thermal shock and abrasion resistance. Bulk density 2.35 to 3.4 g/cm3, apparent porosity 18% maximum.

Q21. What do I specify for continuous casting powder?

Match the powder to casting speed and steel grade, then check the chemistry. Across the five grades, covering low-speed billet, medium-speed bloom, high-speed slab, specialty and peritectic steel, the range is CaO 22 to 45%, SiO2 17 to 56%, basicity ratio 0.8 to 1.3, MgO 0 to 10%, Al2O3 0 to 13%, Na2O 0 to 25% and free carbon 2 to 20%. In the mould it forms three layers: a solid slag layer below 500 °C, a sintered layer at 600 to 900 °C, and a liquid slag layer at 1,300 to 1,500 °C against the steel, 10 to 15 mm thick. Supply comes as granular, powder and extruded forms.

Slide Gate, Nozzles and Ladle Flow Control

Q22. Fired or unburned slide gate plate, and how do I choose between them?

Both are legitimate, and they differ in chemistry and in strength. The fired family covers two material systems: Al2O3-C grades CH-LT70 (alumina 70% or higher, carbon 4% or higher), CH-LT75 (75% or higher, carbon 4% or higher), CH-LT80 (80% or higher, carbon 2% or higher) and CH-LT85 (85% or higher, carbon 2% or higher), and Al2O3-ZrO2-C grades CH-LGT70, CH-LGT75 and CH-LGT80 with ZrO2 4% or higher. Bulk density 2.85 to 3.10 g/cm3, apparent porosity 10 to 12% maximum, cold crushing strength 80 to 120 MPa. The unburned family is CH-MS65, CH-MS75, CH-MS80 and CH-MS85.

Q23. What are the property differences between the fired and unburned slide gate grades?

Unburned slide gate plates are made by high-pressure moulding, low-temperature heat treatment and grinding, with flake graphite, silicon carbide and silicon metal powder added, and they give small sliding surface wear and small injection hole expansion diameter. Grades CH-MS65 and CH-MS75 carry alumina 65% and 75% or higher with carbon 5% or higher, CH-MS80 alumina 80% or higher with carbon 5% or higher, and CH-MS85 alumina 85% or higher with carbon 2% or higher. Bulk density 2.90 to 3.00 g/cm3, apparent porosity 10% maximum for CH-MS65 and CH-MS75 and 8% maximum for CH-MS80 and CH-MS85, cold crushing strength 70 to 100 MPa.

Q24. How do the nozzle and the well block work as a set?

The well block is the stable base masonry built into the ladle or tundish bottom, and the nozzle is the precisely fitted insert in its bore. The combination demands dimensional fit as much as chemistry, because a mismatch is a steel leakage accident. Nozzle grades are CH-SK70, CH-SK75, CH-SK80 and CH-SK85 with alumina 70 to 85% and carbon 3% or higher, in corundum, corundum-spinel and corundum-chrome systems for the well blocks LR-SKZ70, LR-SKZ80 and LR-SKZ85. Bulk density 2.70 to 2.95 g/cm3, apparent porosity 10 to 18% maximum, well block cold crushing strength 40 to 50 MPa, with excellent thermal shock and erosion resistance.

Q25. Ladle filling sand: silica-based or chrome-based?

It depends on the molten steel composition and the residence time, because the sand must not sinter and crust in the well block bore, and it must not let steel penetrate it. The silica-based grade CH-YL80 carries silica 80% or higher at grain size 0.2 to 3.0 mm. The chrome-based grades are CH-YL50 (silica 50% maximum, chrome 25% or higher), CH-YL40 (silica 40% maximum, chrome 30% or higher), CH-YL30 (silica 30% maximum, chrome 35% or higher) and CH-YL20 (silica 20% maximum, chrome 40% or higher) at 0.1 to 2.5 mm, from South Africa chrome ore with lubricant, sintering aid and deoxidiser. Self-flow rate is above 95%.

Q26. How is a ladle purging plug specified, and what does it cost you in downtime?

It is the core functional element of ladle bottom argon blowing, and it is specified on both strength and gas path. Three grades: CH-TQ1 (Al2O3+MgO+Cr2O3 96% or higher, bulk density 3.15 g/cm3 minimum, cold crushing strength 120 MPa minimum), CH-TQ2 (94% or higher, 3.15 g/cm3, 100 MPa) and CH-TQ3 (92% or higher, 3.10 g/cm3, 90 MPa). All three deliver gas permeability 20 to 50 Nm3/h at 0.1 to 1 MPa. Five ventilation types can be built, through-hole, directional slit, directional labyrinth, internal integral and external split, with a matching locking mechanism.

Q27. Do we need a separate desulfurisation product for the ladle, and how is it dosed?

Yes, and it is not a lining material but it runs on the same ladle, so it affects your refractory choice at the slag line. The magnesium-based grades deliver 85 to 95% desulfurisation efficiency, a reaction speed of 5 to 15 minutes and a typical dosage of 0.4 to 1.2 kg per tonne of hot metal, per the Pentaphos industry reference. Five grades cover the duty: Pure Magnesium (Mg 99.8% or higher) for injection systems, a 70:30 magnesium to burnt lime blend for general injection, a magnesium-dolomite blend for high temperature, an enhanced yield mix and a low-fume formula.

Iron Runner, Taphole and Casting House

Q28. How is an iron runner lining built, and what life should I expect?

The working layer uses high-performance Al2O3-SiC-C low-cement or ultra-low-cement castables, and the backing layer uses insulating castables and precast insulation boards; branch runners, skimmers and dams use the matching system. Grade selection follows the zone: CH-TGKJ-70 (alumina 70% or higher, SiC+C 15% or higher) for the main runner and slag skimmer of a large blast furnace, CH-TGKJ-65A (65% or higher, SiC+C 20% or higher) for the runner slag line, CH-TGKJ-65 (65% or higher, SiC+C 8% or higher) for branches and CH-TGKJ-60 (60% or higher, SiC+C 15% or higher) for the slag runner.

Q29. Why is the runner cover made from a lower density castable?

Because the cover is insulation, not a wear surface. It has to hold heat in the runner, so it needs relatively low bulk density, and it has to cope with rapid temperature change when the cover plate is opened and closed. CH-TGG50 (alumina 50% or higher) serves the slag through cover, CH-TGG55 (55% or higher) the branch through cover and CH-TGG65 (65% or higher, SiC+C 15% or higher) the iron runner cover, which is the harshest thermal-cycling zone of the cast house operation. Bulk density 2.2 to 2.6 g/cm3, cold crushing strength 15 to 25 MPa, modulus of rupture 3 to 5 MPa.

Q30. Can we repair the runner without a shutdown and a bake?

Yes, and that is exactly what the firing-free ramming mixes are for. They are manufactured from corundum, high-quality bauxite and silicon carbide, bonded by resins and tar, installed by ramming, and they do not require baking after installation, so the runner goes straight back into service. Grades are CH-TGD-50 (alumina 50% or higher, SiC+C 20% or higher) for the slag trough of small blast furnaces, CH-TGD-55 (55% or higher, SiC+C 15% or higher) for small to medium iron runners and CH-TGD-65 (65% or higher, SiC+C 15% or higher) for medium-size blast furnace runners, on furnaces under 1000 m3.

Q31. Water-based, waterless or environmentally friendly taphole clay: how do I choose?

The binder decides the behaviour. Water-based uses water as the binding agent, moisture content 18.0% and alumina 25% or higher; after 1350 °C for 3 hours it gives bulk density 1.40 to 1.80 g/cm3, cold crushing strength 6.0 MPa, apparent porosity 40% or less and permanent linear change ±1%. Waterless uses tar as the binding agent with moisture below 0.5% and alumina 25% or higher. The environmentally friendly grade switches to a resin binder with alumina 27% or higher and SiC+C 30% or higher, moisture below 0.5%, and after 1350 °C bulk density 1.60 to 2.20 g/cm3, cold crushing strength 8.0 MPa and apparent porosity 35% or less.

Q32. Which waterless taphole clay grade suits my blast furnace?

Four grades, graded by alumina, all holding silicon-carbide-plus-carbon content of 25% or higher. CH-PN20 (alumina 20% or higher) is for the taphole of medium or small-size blast furnaces, CH-PN25 (25% or higher) for large or medium-size, CH-PN30 (30% or higher) for large blast furnaces, and CH-PN35 (35% or higher) is the highest-alumina workhorse grade for the most demanding large blast furnace taphole service. Bulk density 1.8 to 2.10 g/cm3, crushing strength 2 to 3 MPa, permanent linear change ±1% at 1350 °C in coke-bed conditions.

Q33. Why does the blast furnace tuyere need a composite brick?

Because the duty is brutal: tuyere raceway operating temperature above 1,500 °C, high-speed hot blast erosion of 1,000 to 1,500 Nm3/min, K2O and Na2O alkali vapour corrosion, and mechanical stress of 15 to 25 tons of equipment per tuyere assembly. Traditional single-material linings in that zone usually fail within 6 to 18 months. Blast Furnace Tuyere Combined Bricks are pre-assembled from dozens to hundreds of interlocked pieces in three grades: GM-70 corundum-mullite for the tuyere nose, taphole, hot air outlet, three forks and bustle pipe tuyere, ML-60 mullite for the combustion chamber inlet and mixed air, NT-45 clay for the cooler flue tube and turning tube.

Q34. Which materials do the iron mixer and the torpedo ladle need?

The iron mixer buffers and homogenises hot metal, so its lining resists molten iron erosion, thermal cycling and slag corrosion together: Al2O3-SiC Castable for Iron Mixer runs CH-HTJ-L70 (alumina 70% or higher, SiC 12% or higher) for the working lining at side wall and bottom, CH-HTJ-L65 (65% or higher, SiC 12% or higher) and CH-HTJ-L55 (55% or higher, SiC 10% or higher) for top and tapping hole, with cold crushing strength 55 to 60 MPa at 1400 °C. Torpedo ladles take Al2O3-SiC-C brick: CH-ASC18A, CH-ASC18B, CH-ASC20A and CH-ASC20B at alumina 60 to 65% with SiC+C 18 to 20%.

Gunning, Hot Repair and Unshaped Materials

Q35. Gunning, trowelling or ramming: which repair method for which situation?

Match the method to the condition. Gunning is for hot emergency repair. MgO / MgO-C / Forsterite Based Gunning & Trowelling Mixes give CH-TM70 (MgO 60 to 70%), CH-TM80 (MgO 80% or higher) and CH-TMG15 (MgO 65% or higher, CaO 10 to 20%), and the split is deliberate: trowelling mixes for large-area levelling of pitted surfaces in cold state, gunning mixes for emergency repair in hot state. Ramming suits a permanent or semi-permanent cold rebuild. Both products are easy to install, pre-fire and dismantle after use.

Q36. Which gunning mix do I use for converter and ladle cold repair?

Three magnesia grades: PBL70 (MgO 70% or higher) for general converter and ladle cold repair, PBL80 (80% or higher) for standard operating conditions and PBL85 (85% or higher) for demanding service. All three deliver adhesive quality of 85% or higher, which is the number that decides whether the gunned layer actually bonds to the old lining instead of sliding off. Modulus of rupture is 3 to 5 MPa at 110 °C and 6 to 7 MPa at 1500 °C, cold crushing strength 5 to 11 MPa at 110 °C and 20 to 32 MPa at 1500 °C, bulk density 2.3 to 2.5 g/cm3.

Q37. EAF gunning mix: how do I pick a grade for my slag chemistry?

The grade follows the CaO in your slag. CHDPB-87 (MgO 87% or higher) is the highest grade for demanding EAF gunning service, CHDPB-75 (MgO 75% or higher, CaO 10% or lower) is the mid-magnesia variant, and CHDPB-65 (MgO 65% or higher, CaO 30% or lower) is the high-CaO variant for varying slag chemistry conditions. The chemistry difference shows up in volume stability: permanent linear change at 1500 °C for 3 hours runs 0 to 1.5% for CHDPB-87 against -3.0 to 0% for CHDPB-65. Cold crushing strength 15 MPa at 110 °C and 20 to 25 MPa at 1500 °C, bulk density 2.30 to 2.60 g/cm3.

Q38. What is the ladle working layer gunning mix for, and is it really carbon free?

It restores the working layer surface where long molten steel erosion and slag corrosion have thinned it, typically at the slag line and the bottom impact zone, and it keeps the residual thickness balance of the ladle intact. It is manufactured from high-purity corundum and magnesium aluminate spinel, and the wet spraying technique produces no CO2 or CO gas during ladle production and use, so the material can be cycled repeatedly with less waste. Grades CH-GBP85 (alumina 85% or higher) and CH-GBP88 (88% or higher) give apparent porosity 11 to 12% maximum, bulk density 2.80 to 2.90 g/cm3 and cold crushing strength 60 to 70 MPa.

Q39. Carbon-containing or carbon-free hot repairing mix?

The carbon-contained grade gives longer service life; the carbon-free grade is more environment friendly, sinters in a shorter time and flows better. Four grades cover it: CH-DDB78 (MgO-C based, MgO 78% or higher, carbon 5 to 7%), CH-DDB65 (MgO based, MgO 65% or higher, carbon 5 to 7%), CH-DDB85 (MgO based, MgO 85% or higher, carbon-free) and CH-DDB92 (MgO based, MgO 92% or higher, carbon-free). Bulk density after 800 °C for 0.5 hours is 2.2 to 2.6 g/cm3, and MgO content across the family runs 65 to 92%. They are used for ladle bottom and side wall hot repair.

Q40. How do we patch the gap between blast furnace cooling staves and the shell?

With water-free patching mixes, which are manufactured from electric calcined anthracite and high-quality bauxite clinkers bonded by phenolic resin with specialty curing agents added. Two grades cover the two jobs: CH-WYLB is the alumina-rich option with alumina over 92% and iron oxide under 2%, for the gap between the Cooling Stave and the Furnace Shell, and CH-WYLD is the carbon-rich option with carbon over 80% and lower bulk density, for the gap between the Bottom Cover Plate and the Carbonaceous Ramming layer. Both cure at 110 °C for 24 hours, and CH-WYLB reaches cold crushing strength 10 MPa or higher and modulus of rupture 4 MPa or higher.

Steel Plant Engineering and Service

Q41. How is a 200 to 300 ton ladle actually lined, zone by zone?

Refined zoned optimised masonry, not one grade everywhere. The slag line area uses cost-optimised advanced MgO-C brick, because that zone sees the highest temperature and the most severe chemical corrosion at the three-phase boundary of gas, slag and liquid. The sidewall uses Al2O3-MgO-C brick or magnesia-chrome brick, the ladle bottom molten steel impact zone uses low-carbon corundum-spinel brick for erosion resistance, and carbon-free refining uses carbon-free working layer bricks or monolithic castables. The backing is a safety layer insulating castable, with conventional gunning mix hot repair matched to it.

Q42. Which refractories belong in the blast furnace stack, and which in the hearth?

They are different jobs and the stack is the more exposed of the two. The stack working lining mainly uses high-grade high alumina bricks, silicon carbide bricks and special carbon blocks for large blast furnaces, because those have high thermal conductivity and good alkali corrosion resistance. In the lower stack, where thermal load and chemical corrosion are most intense, high-grade SiC bricks or microporous carbon bricks resist zinc vapour and alkali metal penetration. The hearth and bottom use microporous or ultra-microporous large carbon blocks, with ceramic cup technology in corundum-mullite.

Q43. How do I choose checker brick and stove lining material by zone?

Match the material to the dome design temperature in steps. Below 1,300 °C, high-quality high alumina checker bricks. At 1,300 to 1,450 °C, high-grade low creep high alumina brick, supplied as DRL48 to DRL85 with alumina 48 to 85%, where DRL75 and DRL80 are recommended for the combustion chamber and dome and DRL70 is the workhorse grade for the upper checkerwork. At the extreme, 1,450 to 1,500 °C, silica-based or mullite-corundum checker bricks must be used so that no high-temperature creep collapse occurs.

Q44. What is the realistic service life of a hot blast stove lining?

It depends on which brick family you use in which zone, and the two are not interchangeable. The low creep high alumina family covers 48 to 85% alumina with refractoriness of 1,750 to 1,790 °C and a high-temperature load creep rate controlled below 1%. It is the preferred grade for the hot blast stove of small and medium blast furnaces. The low creep andalusite family covers 55 to 70% alumina at refractoriness of 1,790 to 1,810 °C, and the low creep mullite family 56 to 72% alumina at 1,790 to 1,830 °C with 15 to 35 thermal shock cycles at 1,100 °C.

Q45. What is refractory spray coating material, and when would we use it in a steel plant?

It is a high-temperature coating material with extremely fine particles and excellent flowability or pumpability, so it can be sprayed rather than cast or rammed. Its use is sealing, not wear protection. It is applied as a sealing coating on the surface of a new furnace lining, or to renovate a slightly worn surface, and the two things it buys you are protection against initial high-temperature gas flow erosion on the hot face and improved airtightness of the backing insulation materials behind it.

Q46. What do you need from me to engineer and quote a lining?

The drawing and the operating data, not a product name. For a ladle: the ladle drawing, capacity, bottom and side wall lining design, operating temperature and slag chemistry. For a tundish: the tundish drawing, permanent lining design, capacity, continuous casting operating conditions and steel grade. For continuous casting: the machine design, casting speed, steel grade, slab, billet or bloom size and operating temperature. For an EAF: the capacity, bottom or tapping hole design, gunning cycle data and slag chemistry profile. That is what drives grade selection, raw material adjustment and geometry design.

Q47. MgO-C brick or MgO-CaO brick: which one fits my steel grade?

Match the brick to the steel you are making, because the two solve different problems. MgO-C brick, bonded with graphite and phenolic resin, has the best combined thermal shock and slag corrosion resistance in conventional EAF and BOF service, and it is the standard choice for converter working linings and ladle slag lines. The trade-off is a carburisation risk. MgO-CaO brick has no free CaO hydration or carburisation problem, can purify impurities such as sulfur and phosphorus in the molten steel at high temperature, and is the right material for ultra-low-carbon steel, stainless steel and high-cleanliness grades.

Industry Knowledge for Refractory Buyers

How do I read a refractory technical data sheet as a steel plant buyer?

Six numbers decide most ladle and furnace lining purchases. Apparent porosity tells you how connected porosity there is, because every connected pore is a slag and gas path. Bulk density sets heat storage and therefore the thermal gradient behind the lining. Cold crushing strength gives compressive integrity, modulus of rupture gives bending resistance, and refractoriness under load at 0.2 MPa is the only one that describes load-bearing capability at temperature. Permanent linear change is the volume movement the expansion joints must absorb.

Should a ladle working lining be brick or castable?

Brick dominates the ladle working layer because it goes into service faster after a reline and carries no drying or baking requirement on a hot-ladle schedule. Low-cement castable is chosen where a joint-free lining matters more than speed, for example in permanent lining castables and in tundish areas. Gunning mix is not a working layer; it is the repair medium used to restore worn slag line thickness between full relines.

What is the standard brick module, and why does joint count matter?

The standard stock module is 230 x 114 x 65 mm, with modular sizes such as 230 x 114 x 75 mm for thicker working layers. Joint count matters more than brick size itself, because each mortar joint is a potential leak path for slag and a place where thermal stress concentrates. Fewer, larger bricks reduce total joint area, speed installation and improve lining integrity, at the cost of heavier handling and tighter setting-out tolerance.

How much expansion joint allowance does a steel plant lining normally use?

For magnesia and magnesia-carbon the thermal movement is significant, so typical practice allows roughly 1.5% to 2% of the free lining length, which works out around 15 to 20 mm of total joint opening per metre of wall height, with joints commonly spaced 1.0 to 1.5 m apart and staggered between courses. The final number must come from the supplier's expansion data for the actual brick, not from a general rule.

What is the difference between a working lining and a permanent lining in a ladle?

The working lining is the consumable layer that erodes, and it is sized from the measured wear rate of that zone divided by the acceptable loss per campaign. The permanent lining behind it is the safety and insulation layer, sized so a full breach of the working layer does not reach steel within one campaign. In a ladle the working layer is normally only tens of millimetres over a much thicker permanent layer, and permanent lining failure is a safety event rather than a wear event.

How do I calculate annual refractory consumption for a steel plant?

Build it from two streams. Planned relining consumption equals the number of vessels to be lined times the lining area per vessel times the lining thickness times the installed density, plus a waste and damage factor, converted to tonnes and spread over the actual campaign life. Repair consumption equals perimeter times worn area times material applied per gunning event times events per year, plus touch-up gunning mix. Then reconcile the calculated figure against purchase and site issue records, because the gap is where unrecorded loss and rework hide.

Which ladle brick grades resist FeO-rich slag best?

FeO is the most aggressive component against MgO-C brick because it dissolves the periclase and oxidises the graphite. Higher carbon content gives better slag resistance, higher thermal shock resistance and lower porosity, but costs more and reduces thermal conductivity. Grade selection should therefore be made against the actual slag analysis, FeO and MgO/CaO ratio, not by a fixed habit. Where carbon pickup is unacceptable, spinel or carbon-free grades are the alternative.

What is the practical service life difference between working lining grades?

Service life in a ladle is governed by the slag line rather than the average wall, because the slag line sits at the three-phase boundary of gas, slag and metal and takes the highest temperature, the most severe chemical attack and the physical wash at once. Grading the slag line separately from the rest of the working layer and maintaining it with red-hot gunning every 5 to 10 heats is what extends overall campaign life, rather than upgrading the whole lining uniformly.

Cement Kiln Refractory: Zones, Materials, Coating and Service

Questions: 46

Questions in this section
  1. Kiln Zones and Material Selection (6)
  2. Chrome-Magnesia versus Spinel in the Burning Zone (6)
  3. Kiln Coating, Crusting and Blockage (6)
  4. Wear Resistance in the Cooler and Tertiary Air Duct (6)
  5. Insulation, Light Weight and Ceramic Fibre (7)
  6. Cement Plant Engineering and Service (7)
  7. Industry Knowledge for Refractory Buyers (8)

Kiln Zones and Material Selection

Q1. Which refractory goes into which zone of a dry-process cement kiln?

Four zones, four different duties. The burning zone is the heart of the kiln at 1,450 °C direct flame, where clinker forms a liquid phase, so it takes magnesia-chrome or spinel brick that resists corrosion and adheres the kiln coating for self-protection. The transition zone swings between rapid heating and cooling and repeatedly sheds and rebuilds its coating, so it needs thermal-shock-resistant silicon mullite brick. The cooler takes high-hardness clinker falling at high speed, so it needs ultra-wear-resistant SiC or high alumina brick. The preheater works in an alkali fog of low-melting-point salts, so it takes alkali-resistant brick and anti-crust castable.

Q2. What does a complete turnkey refractory package for a cement line cover?

The material matrix covers every inch of the high-temperature area: high alumina bricks, magnesia-chrome bricks, spinel bricks, anti-crust castables for the preheaters, alkali-resistant castables, high-strength wear-resistant castables for the kiln mouth, erosion-resistant castables for the tertiary air duct, and special burner coal pipe castables.

In practice that means one source for the preheater, calciner, burning zone, transition zone and cooler, with type selection, raw material adjustment and geometry design matched to your own kiln drawing and operating conditions instead of a mixed basket of mills with incompatible specs.

Q3. How do I pick the right high alumina brick grade for the kiln lining?

Match the grade to the service temperature and the load carried. Four chemistry grades are available: CH-LZ48 at 48% Al2O3, CH-LZ55 at 55%, CH-LZ65 at 65% and CH-LZ75 at 75%. Across the range, cold crushing strength is 40 to 54 MPa at normal temperature, apparent porosity is no more than 22 to 23%, load softening temperature is 1,420 to 1,520 °C and refractoriness is 1,750 to 1,790 °C, while permanent linear change stays within plus or minus 0.1 to 0.4% after two hours at 1,450 to 1,500 °C. Grade selection follows the zone map rather than a single house grade.

Q4. Which castable for the kiln ends, the kiln door and the hood?

The kiln door appropriative castable comes as CH-YKJZ70 at 70% Al2O3 and CH-YKJZ75 at 75%, both rated to a 1,600 °C maximum service temperature, with cold crushing strength of 80 to 100 MPa, modulus of rupture of 10 to 13 MPa and permanent linear change within plus or minus 0.5% after three hours at 1,400 °C.

For the rotary kiln front kiln mouth, disintegration furnace and kiln hood, the cement bonded castable grades GLJZ-85, GLJZ-70, GLJZ-60, NTJZ-50 and NTJZ-42 cover 1,640 to 1,780 °C refractoriness, with 20 to 35 MPa cold crushing strength at 110 °C and a test temperature after burning of 1,350 to 1,500 °C.

Q5. What protects the burner coal injection pipe?

The coal injection pipe needs its own grade because it combines thermal shock, corrosive gas flow and continuous exposure. Three chemistry grades are offered: CH-PJZ68 at 68% Al2O3, CH-PJZ72 at 72% and CH-PJZ78 at 78%, built on andalusite, corundum-mullite, composite material and a differential combination of activated aluminum powder. Bulk density is 2.6 to 2.8 g/cm³, modulus of rupture is 8 to 12 MPa, cold crushing strength is 60 to 90 MPa and permanent linear change is within plus or minus 0.5% after three hours at 1,400 °C, with good thermal shock stability, high corrosion resistance and stable volume.

Q6. Which castable for the calciner and the carbon calcined rotary kiln?

The carbon calcined rotary kiln range is CH-JZ45 at 45% Al2O3, CH-JZ60 at 60% and CH-JZ70 at 70%, with bulk density 2.4 to 2.6 g/cm³, cold crushing strength of 35 to 80 MPa and permanent linear change at most 0.01 to 0.02% after curing at 110 °C.

The carbon baking furnace family adds CH-TLZ45, CH-TLZ60 and CH-TLZ70, with maximum service temperatures of 1,400, 1,450 and 1,500 °C, alongside the TLD and TLQ grades at 1,400 to 1,450 °C. Both families serve the calcination and roasting of cement, limestone, magnesia, ilmenite and nonferrous metal ore, at the rotary kiln mouth, calcination zone, cooler and feed nozzle.

Chrome-Magnesia versus Spinel in the Burning Zone

Q7. What refractories are used in the burning zone, and how long do they last?

Three material families are in service: direct-bonded magnesia-chrome bricks, high-quality magnesia-alumina spinel bricks, and dolomite bricks. All of them work by adhering the kiln coating, so it is the coating, not the brick, that resists the liquid clinker phase. On life, magnesia-chrome brick usually runs 6 to 12 months, while high-quality dolomite or spinel bricks reach 8 to 18 months. The comparison therefore belongs in months per lining campaign on the hottest zone of the kiln, where a shutdown costs the most.

Q8. Should a new dry-process kiln use magnesia-chrome or magnesia-spinel brick?

Magnesia-alumina spinel brick, if the kiln is new today. Magnesia-chrome brick was once the absolute dominator of the burning zone: it is co-sintered from high-purity magnesia and chrome ore, and its surface periclase-spinel network hangs a strong and stable cement clinker coating that protects the brick body from further erosion. The problem is the waste stream, because hexavalent chromium in discarded magnesia-chrome brick is a strong carcinogen and faces strict environmental bans. Spinel brick is manufactured from high-purity magnesia and synthetic magnesia-alumina spinel fine powder, so it completely eliminates the toxic hexavalent chromium released from discarded traditional magnesia-chrome brick.

Q9. What does the kiln coating actually do for the burning zone brick?

It is the primary line of defence. Under the erosion of high-temperature liquid clinker, the surface periclase-spinel network of the brick hangs a strong and stable cement clinker coating over the brick body, and that layer is what protects the brick from further erosion. This is why burning zone materials are selected on coating adhesion first. Where the coating does not hold, the transition zone with its frequent coating shedding and coating rebuilding is specified on thermal shock spalling resistance instead, because there the brick itself has to survive the cycle.

Q10. Does going chrome-free cost coating adhesion or corrosion resistance?

No. Magnesia-alumina spinel brick achieves equally excellent levels of coating adhesion, thermal shock resistance and chemical corrosion resistance, and through micro-thermomechanical performance optimisation its comprehensive service performance has fully matched, or even exceeded, magnesia-chrome brick. It is the first choice for the burning zone of modern new dry-process cement kilns and the complete substitute for chrome-magnesia in the chrome-free era. Specify it against the same measured numbers you used for the chrome grade, so the comparison stays honest.

Q11. Where does dolomite brick fit in the burning zone?

Dolomite brick belongs in the same short list as magnesia-chrome and spinel: it is one of the three materials used in the burning zone and it also adheres the kiln coating for self-protection. On life it sits with the chrome-free options, with high-quality dolomite and spinel bricks reaching 8 to 18 months against the 6 to 12 months typical of magnesia-chrome brick. The decision is therefore not chrome versus no chrome, it is a 12-month class material against a 12 to 18-month class material, decided by the grade installed and by how the coating behaves in your own kiln.

Q12. What does switching to chrome-free mean for waste and for spare parts supply?

Two practical consequences follow. First, waste handling: hexavalent chromium in discarded magnesia-chrome brick faces strict environmental bans, while a spinel burning zone removes the toxic Cr6+ released from discarded traditional magnesia-chrome brick from your demolition and disposal stream. Second, supply continuity: supply chain de-globalisation is pushing regional giants to strengthen localised procurement of spare parts to prevent supply interruption risks, which favours a single source covering the whole line over spot buys from different mills.

Kiln Coating, Crusting and Blockage

Q13. What actually causes crusting and blockage in a cyclone preheater?

It is condensation of volatiles, and the chemistry usually starts in the raw meal and the fuel. Volatile compounds such as alkalis including K2O and Na2O, plus sulfur and chlorine, volatilise in the high-temperature zone of the kiln and then condense when the flue gas rises into the lower-temperature preheater system. Those condensed molten salts are extremely sticky, and once they adsorb large amounts of dust they form hard crusts and blockages on the cylinder wall, seriously affecting ventilation. The preheater therefore runs permanently in what is effectively an alkali fog of low-melting-point salts.

Q14. How does anti-crust castable solve it, and which grade?

It works by making the surface impossible to grip. The anti-crust castable grades are rich in silicon carbide: CH-KJZL55 gives SiC+SiO2 of at least 55% with a maximum service temperature of 1,300 °C, and CH-KJZL60 gives at least 60% with 1,400 °C. In the high temperature state the surface oxidises to form a smooth, non-porous glassy micro-film, so the raw meal powder carrying large amounts of alkali salts cannot adhere.

Bulk density is 2.4 to 2.5 g/cm³, cold crushing strength is 60 to 80 MPa, modulus of rupture is 8 to 11 MPa and permanent linear change is within plus or minus 0.4% after three hours at 1,100 °C.

Q15. Which alkali-resistant brick type for the preheater, decomposition furnace and vault?

The Normal Type, Al2O3 25 to 30% and SiO2 65 to 70%, covers general preheater and decomposition furnace service; the High Strength Type, same chemistry, is for higher-demand preheater, decomposition furnace and tertiary air duct duty. The Insulated Type, SiO2 60 to 70%, serves insulated lining, and the Vault Type, Al2O3 30 to 35% and SiO2 60 to 65%, serves the kiln vault.

The protection is chemical: the brick reacts with alkaline oxide to form a high-viscosity glass phase that covers the surface and blocks alkaline slag infiltration. Refractoriness is 1,650 to 1,710 °C and refractoriness under load at 0.2 MPa is 1,250 to 1,400 °C.

Q16. Which castable for the kiln door hood and the preheater cones?

These positions take the most direct contact with strongly alkaline raw meal and flue gas carrying K2O, Na2O and alkali chloride vapours, so the high strength alkali resistant castable is specified there. Two grades: CH-NJZ48 with Al2O3 at maximum 48% and SiO2 at minimum 50% for general service at 1,300 °C, and CH-NJZ45 with Al2O3 at maximum 45% and SiO2 at minimum 53% for higher-demand service at 1,350 °C. Both deliver alkali resistance grade 1 to 2, bulk density 2.2 to 2.4 g/cm³, cold crushing strength 60 to 70 MPa and permanent linear change within plus or minus 0.4% after three hours at 1,100 °C.

Q17. How does burning waste fuel change the preheater risk?

It raises it sharply. To compress coal costs, plants feed large amounts of RDF (compressed domestic waste), sawdust agricultural biomass and even waste car tyres into the kiln, and the price is that large amounts of hidden sulfur (S), chlorine (Cl) and alkali metals (K, Na) are violently released, forming highly penetrating and corrosive acid-alkali toxic fog, while heat value fluctuations bring strong thermal shock damage on top.

That is why cement plant cost optimisation through alternative fuels is now described as causing soaring alkali load in kilns and urgently requiring upgraded super alkali-resistant linings: high-density alkali-resistant castables plus anti-blocking, anti-crust special materials in the affected zones.

Q18. Should the whole preheater be lined with the same material?

No, and the reason matters because the failure mode changes with the part. The cyclone preheater cutting slope, the rising flue and the preheater cone take anti-crust castable, because the glaze layer that forms in the high temperature state is what stops the sticky meal from adhering there. The wider preheater and the decomposition furnace shell take alkali-resistant brick, whose high-viscosity glass phase blocks the surface pores against alkaline slag infiltration. The kiln door hoods and the most exposed preheater cones take the high strength alkali resistant castable.

Wear Resistance in the Cooler and Tertiary Air Duct

Q19. Which material for the tertiary air duct?

A special wear-resistant castable, not a general kiln grade. The tertiary air duct appropriative castable comes in three chemistry grades: CH-FJZ65 at 65% Al2O3 with a 1,450 °C maximum service temperature, CH-FJZ75 at 75% with 1,500 °C, and CH-FJZ80 at 80% with 1,600 °C. The formula is a composite of high-purity corundum and silicon carbide wear-resistant aggregates, giving diamond-like wear resistance and erosion resistance.

Bulk density is 2.6 to 2.8 g/cm³, modulus of rupture 11 to 13 MPa, cold crushing strength 90 to 120 MPa and permanent linear change within plus or minus 0.5% after three hours at 1,400 °C, with anti-flushing behaviour and no cracking.

Q20. Why does the tertiary air duct lining wear faster than the kiln lining?

Because of the gas. Wind speed in the tertiary air duct is extremely fast, and it carries a large amount of highly abrasive high-temperature clinker dust, so the lining is under continuous particle erosion rather than slow chemical attack. The specification that follows from that is a special high-strength, spalling-resistant, high-temperature wear-resistant castable, and heat-resistant steel anchors are often welded inside the duct to strengthen the structure of the lining. Spec a cheaper general-purpose castable there and it will be swept away long before the kiln body needs attention.

Q21. Which brick for the grate cooler?

Silicon carbide brick, or special high alumina wear-resistant brick, with high-strength wear-resistant castable of the same material wherever a joint-free surface is needed. The cooler faces strong erosion and abrasive wear from large amounts of high-hardness, high-speed falling clinker particles. SiC brick uses artificially synthesized silicon carbide as the core raw material and is characterised by extremely high thermal conductivity, unparalleled high-temperature wear resistance and extremely strong resistance to alkali vapour corrosion, which makes it the ultimate solution for wear-resistant areas of cement grate coolers and cyclone preheater linings.

Q22. Is silicon mullite better than high alumina brick in the cooling zone?

In the transition and cooling zones it is the better choice, and it was developed for those positions. Silicon mullite brick combines high-grade bauxite clinker with high-quality silicon carbide, fired at high temperature, so it takes the corrosion resistance of silicon carbide and the high strength of alumina. Its long-life performance far exceeds traditional high alumina brick in the transition zone and cooling zone of cement kilns. Three grades are offered, CH-GMZ65, CH-GMZ63 and CH-GMZ60, all with minimum refractoriness of 1,790 °C, cold crushing strength of 80 to 95 MPa, apparent porosity of 20 to 21% maximum and refractoriness under load at 0.2 MPa of 1,550 to 1,680 °C.

Q23. Where do phosphate bricks fit, and how do I choose the grade?

Phosphate brick is the answer where the lining tends to loosen and fall out: the cement kiln transition zone, the kiln mouth, the kiln door cover and the cooler inner lining. It combines higher strength and good wear resistance with alkali resistance better than clay bricks and high alumina bricks, plus good thermal shock resistance and a high load softening temperature. Three grades are offered: CH-PZ75, a phosphate combined wear-resistant brick at 75% Al2O3; CH-PA75 at 75% Al2O3 for higher-demand transition zone service; and CH-PT80 special phosphate brick at 80% Al2O3 for the most demanding duty, with a lightweight option at 55% Al2O3 for insulated lining.

Q24. Is there a castable for the kiln mouth and calcination zone that handles acid and alkali attack?

Yes, the anti-seepage castable CH-TLD, with Al2O3 at maximum 35%. It is fitted to the rotary kiln kiln mouth, the calcination zone, the cooling machine and the feed nozzle, and to calcination and roasting of cement, limestone, magnesia, ilmenite and nonferrous metal ore, with strong acid and alkali corrosion resistance. It reacts with electrolyte alkali metal ions in the high temperature state to form a glaze layer that blocks penetration. Bulk density is minimum 2.1 g/cm³, cold crushing strength minimum 50 MPa at 110 °C and 60 MPa at 1,000 °C, thermal conductivity at most 0.5 W/m·K at 350 °C and 0.7 W/m·K at 650 °C.

Insulation, Light Weight and Ceramic Fibre

Q25. What should sit behind the hot face, and does it affect shell temperature?

Behind the hot face, use a low-density product and let the working layer take the abrasion. Lightweight refractories include lightweight castables, insulating refractory bricks and nano-microporous insulation boards, which act as a firewall blocking heat outflow. The nano-microporous board reaches a thermal conductivity of 0.025 W/m·K or lower, so only a very thin layer replaces several times the thickness of traditional insulation bricks.

For very high-temperature service the alumina hollow sphere products CH-KXQ88, CH-KXQ98 and the CH-KXQ98 Sialon grade at 9.8% ZrO2 reach maximum service temperatures of 1,650 to 2,200 °C, with load softening temperature of 1,650 to 1,700 °C at 0.2 MPa.

Q26. Which insulating brick should I specify: clay, high alumina or mullite?

The temperature decides. Clay insulating brick, in NG-0.5 up to NG-1.0 grades by bulk density, is the lower-temperature option: thermal conductivity at most 0.18 to 0.50 W/m·K at an average 350 °C and load softening of 1,160 to 1,300 °C at 0.1 MPa, with Fe2O3 at most 2.0 to 2.5%. High alumina insulation brick CH-LG0.6, CH-LG0.8 and CH-LG1.0 holds at least 48% Al2O3 and raises the ceiling to 1,300 to 1,380 °C. Mullite insulation brick, in eight JM23 to JM28 grades, reaches the same ceiling with bulk density as low as 0.6 to 1.2 g/cm³, and can contact flame directly as a working layer.

Q27. Where do light weight silica brick and sillimanite brick fit?

Light weight silica brick CH-QZ1.2 carries at least 91% SiO2 with refractoriness of 1,670 °C and load softening start of 1,520 °C at 0.1 MPa; its many pores improve thermal shock resistance but cost compressive strength, slag resistance and corrosion resistance compared with ordinary silica brick. Sillimanite brick CHGX-60, at 60 to 65% Al2O3 and 30 to 35% SiO2, is the option where the surface is not eroded by molten liquid, with apparent porosity of 18% maximum, cold crushing strength of 30 MPa minimum, load softening of 1,550 °C at 0.2 MPa and thermal shock resistance of 30 cycles at 1,100 °C water cooling.

Q28. When do I use a light weight castable and when a light weight gunning mix?

Castable where the lining is formed and shelled, gunning mix where access is poor. The light weight castable family runs seven QJ grades from CH-QJ0.5 at 0.5 plus or minus 0.1 g/cm³ up to CH-QJ1.8 at 1.8 plus or minus 0.1 g/cm³, with cold crushing strength of 1.5 to 8 MPa and maximum service temperatures from 700 to 1,350 °C.

Gunning grades CH-QP0.7, CH-QP1.0 and CH-QP1.4 sit at 0.75, 1.1 and 1.5 plus or minus 0.1 g/cm³, with cold crushing strength of 2 to 6 MPa and thermal conductivity at most 0.30 to 0.54 W/m·K at 800 °C hot side. They are sprayed or painted, with low rebound.

Q29. How hot can ceramic fibre go, and which format for which job?

Three temperature classes exist: ordinary type at 1,050 °C, zirconia-containing type at 1,430 °C and polycrystalline alumina high-end fibre at 1,600 °C, with extremely low bulk density of only 64 to 192 kg/m³. Format follows the job.

Blankets (CH-XWT40, XWT45, XWT48, XWT50, XWTZ15) run 1,000 to 1,350 °C with volume density 95 to 160 kg/m³ and thermal conductivity at most 0.14 to 0.28 W/m·K; boards (CH-XWK) are denser at 200 to 600 kg/m³; felts (CH-XWZ) at 150 to 250 kg/m³ are the flexible joint and gasket material; modules (CH-XWK) are pre-compressed blocks; bulk (CH-XWM) is loose fill; shaped pieces (CH-XWJ) are vacuum-moulded burner blocks and furnace doors.

Q30. Can ceramic fibre be cast into a monolithic lining?

Yes. The ceramic fibre castable grades CH-XWC06, CH-XWC08, CH-XWC10, CH-XWC12 and CH-XWC15 carry Al2O3 of at least 20%, 25%, 30%, 35% and 35%, with Al2O3+SiO2 of at least 80%, and they combine good flowability, easy installation, low conductivity and volume stability. Service temperature is 600 to 1,100 °C depending on grade, thermal conductivity is at most 0.16 to 0.28 W/m·K, permanent linear change is at most 1.0% after three hours at 600 °C and cure time is no more than 10 hours, with 25 kg bags. Applications include heating furnaces, reforming furnaces, hydrogen furnaces, firing blocks, burning blocks and molten aluminium collector and groove service.

Q31. What is bubble alumina, and when is it better than a conventional insulating brick?

Bubble alumina, also called alumina hollow sphere, is a hollow sphere aggregate made from high purity Al2O3 by high temperature melting and atomization. The high purity grade carries Al2O3 of at least 99% with SiO2 at most 0.2% and Fe2O3 at most 0.1%. Stacking density is 0.4 to 1 g/cm³, size is 0 to 7 mm and the maximum working temperature is 1,825 °C.

Baked into brick it gives bubble alumina brick grades CHSAH99 at 99.3% Al2O3, CHAH99 at 99%, CHAH90 at 90% and CHAH85 at 85%, with bulk density 1.4 to 1.9 g/cm³ and cold crushing strength of 12 to 18 MPa.

Cement Plant Engineering and Service

Q32. How do we monitor lining condition from the shell, and when do we stop?

Shell surface temperature is the most direct early warning indicator for the residual thickness of the internal lining, and scanning the rotating steel shell costs nothing. The normal operating target of a new dry-process cement kiln is a burning zone shell temperature below 350 °C. If the measured temperature at one point suddenly crosses the 350 °C warning line or even turns red, it means the working lining there has burned through and peeled off, and high-temperature clinker is burning the remaining thin permanent insulation layer or even the external steel shell. Local abnormal temperature rise with red kiln signs means stopping the kiln immediately for repair.

Q33. What do you need from us to produce a tailored lining proposal?

Engineering starts with your drawings rather than our catalogue. Send the cement kiln drawing, the lining design, the kiln capacity and the operating temperature data, and the engineering team in Xinmi City, Zhengzhou, Henan, China provides a free consultation, on-site technical support and a tailored formulation proposal with optimised type selection, raw material adjustment and geometry design for your specific service conditions.

The formulation is adjusted to match: Al2O3 content, SiO2 content, Fe2O3 content, the raw material formulation and the additive or binder system can all be moved against your kiln service temperature and alkali resistance conditions, including the grade and the size of the piece.

Q34. Can we get samples before committing to a bulk order?

Yes. For standard conventional shaped blocks and bulk powder categories a full set of small samples is sent free of charge, with the volume package usually 5 kg or less, and you only bear the meager international express postage. Where the sample involves an extremely demanding or proprietary formula customised high-end development, the R&D centre may charge a special mould opening formula R&D fee, but that fee is fully offset and returned in cash against the bulk production order you subsequently place. All international air freight costs are advanced and settled by the requesting party, in line with international practice.

Q35. Do you supply bauxite, refractory cement and clay as separate products?

Refractory grade bauxite, also called calcined bauxite, comes in five grades: RK70 at 70% Al2O3 up to RK87 at 87%, with Fe2O3 at most 1.5 to 2% and CaO+MgO and K2O+Na2O each at most 0.4 to 0.6%. Bulk density is 2.95 to 3.35 g/cm³, supplied as 0-0.3 mm to 5-8 mm aggregate and 100, 200 or 325 mesh powder.

The binder is the calcium aluminate refractory cement: A600 at 50% Al2O3 minimum, A700 at 50 to 60%, A900 at 53.5% minimum and CA-70 at 68.5 to 70.5%, with initial setting 45 to 180 minutes and 24-hour cold crushing strength 40 to 72 MPa.

Q36. Which mortar and clay do we use to joint the lining?

Six refractory clay grades cover clay brick and high alumina brick work: CH-NN38 at 38% Al2O3 with 1,630 °C refractoriness, CH-NN42, CH-NN45, then CH-LN55, CH-LN65 and CH-LN75 at 75% Al2O3 with 1,790 °C, all with a modulus of rupture of at least 1 MPa after curing at 110 °C for 24 hours. For dedicated high alumina brick masonry, three high alumina refractory mortar grades CH-LN55, CH-LN65 and CH-LN75 give 1,770 to 1,790 °C refractoriness, and seven general refractory mortar grades from CH-GA88 to CH-GT70 give 1,500 to 1,690 °C with hardening time of 60 to 180 seconds and adhesive strength of at least 1 MPa.

Q37. Is refractory supply secure for the next few years, and where do you export?

Supply is large and growing: China alone has about 25 million tons a year of capacity, and the global market stood at about USD 39.1 billion in 2026, growing at about 6 to 8% a year toward about USD 59 billion by 2031. The 2030 targets include cutting manufacturing-side carbon emissions by 30% and lifting high-end special products above 50% of output.

Chinese exports already reach the Indian market, the Southeast Asian transfer circle of Vietnam, Indonesia, Thailand and Malaysia, the Middle East with Saudi Arabia, the UAE and Iran, Africa with Egypt, Morocco and Nigeria, Europe with Russia, Turkey and Italy, and South America with Brazil, Chile and Argentina.

Q38. Do you supply the shaped ancillaries and the adjacent kiln product lines?

Shaped ancillaries come from the same plant: anchor brick CH-MG48 and CH-MG55 for furnace roof and suspended lining, frame brick CH-BK55 to CH-BK65 for burner block connection, and hanger brick CH-DG1.8 and CH-DG2.0 for charge gate, discharge gate and partition work.

Adjacent kiln and furnace lines run on the same quality system: DRI rotary hearth and reduced nickel kiln castables in the CH-HZ series, arc furnace cap castables DLD75 to DLD92, special silicon patching material for glass kiln and coke oven repair, and slag and abrasion resistant furnace bottom castables CH-BLN70 to CH-BLN80 with a water requirement of 5 to 7%.

Industry Knowledge for Refractory Buyers

How do I select refractory for each zone of a cement rotary kiln?

The kiln has four distinct consumption zones and each needs a different material. The burning zone, at 1,450 °C direct flame, takes the highest grade magnesia-chrome or magnesia-alumina spinel brick that can hold a stable kiln coating. The transition zone cycles hot and cold and suffers coating shedding, so it takes thermal-shock resistant grades such as silicon mullite. The grate cooler takes high-abrasion silicon carbide or high alumina wear brick against falling clinker. The preheater system runs in an alkali-rich atmosphere and takes anti-crust castable and alkali-resistant brick.

Should the burning zone use chrome-magnesia or magnesia-alumina spinel?

Chrome-magnesia has excellent chemical corrosion resistance and strong coating adhesion, which is why it is the traditional burning zone standard, but the hexavalent chromium released when the brick is discarded faces strict environmental restrictions. Magnesia-alumina spinel is the chrome-free alternative and, through micro-thermomechanical optimisation, has matched or exceeded chrome-magnesia in service performance. It is now the default in modern new dry-process lines.

How does kiln coating form, and why does it matter?

Coating is a protective silicate layer that forms when the hot face reacts with the clinker and binds to the brick, and it is the primary defence of the burning zone lining. Correct heat transfer and a stable coating let the shell temperature stay below the 350 °C operating red line. Where the coating is chemically unstable it repeatedly sheds and rebuilds, and each cycle strips lining material away from the hot face.

What causes crusting and blockage in a cyclone preheater?

Volatile compounds including alkalis, sulphur and chlorine from the raw meal and alternative fuels volatilise in the hot zone and condense when the flue gas rises into the cooler preheater system. These condensed molten salts are extremely sticky and, after adsorbing dust, form hard crusts that block the cylinder wall and choke the system. Anti-crust castable works by forming a smooth, non-porous glassy micro-film on the surface that raw meal cannot adhere to.

How much does alternative fuel affect kiln lining life?

It is close to a double-edged effect. Because it cuts coal cost, plants burn RDF, sawdust biomass and even waste tyres, and the price is that hidden sulphur, chlorine and alkali metals are released in quantity, forming a highly penetrating and corrosive acid-alkali fog. Heat value fluctuation also brings severe thermal shock damage. The defence is comprehensive: upgraded high-density alkali-resistant castable and anti-blocking anti-crust materials across the preheater.

What shell temperature should a cement kiln run at?

Below 350 °C at the burning zone is the operating red line for new dry-process kilns. Shell surface temperature is the most direct early warning indicator of lining thickness, because once it crosses 350 °C and turns red, the remaining permanent insulation is being burnt through and the steel kiln shell itself can begin to deform and fail. Regular scanning of the shell is a continuous health check on the refractory.

How do I choose between a dense and a light-weight castable in a kiln lining?

Position decides it. The working layer takes the dense grade because it carries the abrasion and the thermal load. Behind it, a light-weight or insulating castable of 300 to 600 kg/m3 volume density is used for the thermal barrier, sometimes combined with microporous board. A kiln wall built dense throughout is heavier, more expensive and loses more heat than the design needs.

What are the standard refractory grades used in a cement kiln?

The catalogue grades map onto kiln positions. High alumina brick covers general lining and the transition zone. Magnesia-chrome and magnesia-alumina spinel brick are reserved for the burning zone. Silicon mullite brick serves the transition zone where coating shed and rebuild is severe. Silicon carbide brick and high alumina wear brick line the cooler and tertiary air duct. Alkali-resistant and anti-crust castable protect the preheater cone, and high strength wear-resistant castable protects the kiln mouth.

Glass Kiln Refractory and AZS

Questions: 42

Questions in this section
  1. AZS Grade Selection and Chemistry (6)
  2. Glass Furnace Crown and Silica Brick (5)
  3. Ramming Mass and Sealing Layers (4)
  4. Refractory Ball and Insulating Products (6)
  5. Hot Repair of Fused AZS (6)
  6. Glass Furnace Engineering and Service (7)
  7. Industry Knowledge for Refractory Buyers (8)

AZS Grade Selection and Chemistry

Q1. What actually changes in the brick when you go from AZS-33# to AZS-41#?

AZS is the national standard abbreviation, and it comes from the Al₂O₃-ZrO₂-SiO₂ ternary phase diagram the brick is built on: Al₂O₃ takes A, ZrO₂ takes Z and SiO₂ takes S. The grade number is the zirconia fraction. AZS-33# carries ZrO₂ 32-36% with SiO₂ maximum 16%, AZS-36# carries ZrO₂ 35-40% with SiO₂ maximum 14%, and AZS-41# carries ZrO₂ 40-44% with SiO₂ maximum 13%. The AZS-41# brick is internally filled with a eutectic structure of tightly interwoven corundum and baddeleyite, and its exudation temperature of the vitreous phase is minimum 1,400 °C, the same as the other two grades.

Q2. What chemical limits should I check on the AZS certificate before I accept a delivery?

Check the full specification, not only the headline ZrO₂ figure. SiO₂ is capped at 16% on 33#, 14% on 36# and 13% on 41#. Na₂O is capped at 1.45% on 33# and 36#, and 1.30% on 41%. Fe₂O₃+TiO₂ is maximum 0.30% on all three, and the combined Fe₂O₃+TiO₂+CaO+MgO+Na₂O+K₂O is maximum 2.00%. These same chemistry limits are what our engineers adjust against your service temperature and erosion conditions, together with the raw material formulation and the casting type, before a grade is fixed for your furnace.

Q3. Does the casting type - PT-QX, ZWS or WS - change what I have to specify?

Yes, because volume weight is reported per casting type as well as per grade. On AZS-33# the minimum volume weight is 3.45 g/cm³ for PT-QX, 3.60 g/cm³ for ZWS and 3.70 g/cm³ for WS. On AZS-36# it is 3.45, 3.70 and 3.80 g/cm³, and on AZS-41# it is 3.55, 3.85 and 3.95 g/cm³. When you compare two bids, check the casting type as well as the grade code, otherwise you are comparing two different products at the same headline ZrO₂ number.

Q4. If glass contamination from the brick is my worry, which grade and which property do I specify?

Bubble precipitation rate, measured at 1,300 °C for 10 hours, is maximum 2.0% on 33#, 1.5% on 36# and 1.0% on 41%, so the higher grades keep fewer bubbles out of your glass. But vitreous phase seepage amount at 1,500 °C for 4 hours runs the other way: maximum 2.0% on 33#, and maximum 3.0% on both 36# and 41%. Exudation temperature of the vitreous phase is minimum 1,400 °C on all three grades, which is how far the glass phase can be heated before it bleeds out. If bubbles are your concern, buy up. If bleeding glass phase is your concern, the cheapest grade may be right.

Q5. Why do bulk density and apparent porosity matter so much when I compare AZS bricks?

Porosity is the path the melt takes into the brick, and bulk density tells you how much solid material sits behind that path. Bulk density is minimum 3.75 g/cm³ on AZS-33# with apparent porosity maximum 1.5%, minimum 3.80 g/cm³ on AZS-36# with apparent porosity maximum 1.0%, and minimum 3.95 g/cm³ on AZS-41# with apparent porosity maximum 1.0%. The brick is cast as a dense block, and that is what produces those low porosity figures and keeps the corrosion rate down.

Q6. Does the zirconia logic carry over to a zirconium sizing nozzle, or is that a separate world?

It is a separate product family and the zirconia numbers are not comparable. The sizing nozzle and zirconium core sub-systems run on 13 DJX chemistry grades, X1 to X13, covering ZrO₂ content from 70% to 95%, while the outer coat sub-system uses 6 DJW grades, W1 to W6, at ZrO₂ minimum 65%-75% with carbon content. The 70%-85% grades are the standard variants, 90%-93% are the higher-quality variants and 95% is the highest-quality variant, against 40-44% on AZS-41#. Bulk density is minimum 3.8 to 5.5 g/cm³ for the nozzle and core.

Glass Furnace Crown and Silica Brick

Q7. What failure modes should I expect in a silica crown, and how does the brick chemistry cause them?

Silica brick is mainly tridymite and cristobalite with a small amount of residual quartz and glass phases, and that structure sets the failure modes. Its load softening start temperature is 1,620 to 1,670 °C, so above that the crown creeps. Its thermal shock stability is inherently low, with water heat exchange for only 1 to 4 cycles, so a fast heat-up spalls it. Heated to 1,450 °C it expands 1.5 to 2.2% in total volume, which tightens the joints but also crowds the lining.

Q8. Which silica brick grade should I use in the crown, and what do the three grades cost in strength?

Three grades, differing in silica content, refractoriness and cold crushing strength. CH-GZ95 has silica 95% or higher, refractoriness 1,710 °C and cold crushing strength 29.4 MPa or higher, and it is the grade for the most demanding industrial furnace positions. CH-GZ94 has silica 94% or higher, the same 1,710 °C refractoriness and 24.5 MPa or higher, for intermediate temperature zones. GZ-93 has silica 93% or higher, refractoriness 1,690 °C and 19.6 MPa or higher, for cost-effective cooler zone lining.

Q9. How do I bake a silica crown through the quartz transformation without cracking it?

Do it slowly and under a reducing atmosphere. Silica is slow-calcined at 1,350 to 1,430 °C so that the quartz converts to scaly quartz with the appropriate mineralizer addition, rather than being shocked through the transformation. From there the brick reaches about 1.5 to 2.2% of total volume expansion at 1,450 °C, which makes the masonry joints tight and ensures good air tightness and structural strength of the lining. Do not rush the ramp: thermal shock stability is low, with water heat exchange for only 1 to 4 cycles, and a fast heat-up spalls the brick.

Q10. Can I repair cracks in the crown masonry without relining the whole crown?

Yes, because the expansion and shrinkage characteristics of a silica-based ramming mass are completely consistent with silica bricks, so the patch works with the surrounding masonry instead of fighting it. It is the standard tool for hot or cold sealing repair when cracks or gaps occur in the silica brick masonry of a glass furnace crown. Four grades are available: DDL-1 Silica, silica 98% or higher and refractoriness 1,700 °C; DDL-2 Quartz, silica 98% or higher and refractoriness 1,750 °C; DDL-3 Silica-SiC, silica 98.5% or higher with SiC 5% or higher; and DDL-4 Quartz-SiC, silica 98.5% or higher with SiC 5% or higher and refractoriness 1,750 °C.

Q11. Do I need a different silica brick for a hot blast stove vault and checker than for a glass furnace?

Yes, and the geometry grade carries the difference. The Vault brick grade is engineered for the hot blast stove vault and combustion chamber, with cold crushing strength of 35 MPa or higher. The Checker brick grade targets the checker regenerator, with a low creep rate under 0.8% at 0.2 MPa, 1,550 °C, 50 hours, and thermal linear expansion under 1.26% at 1,500 °C. Both hold silica of 95% or higher and bulk density of 2.35 g/cm³ or higher, with load softening start temperature of 1,620 to 1,670 °C.

Ramming Mass and Sealing Layers

Q12. Which ramming mass do I use for the sealing layer and the frit bath kiln pool?

Fused AZS ramming mass is the grade built for glass furnace and frit bath kiln sealing layer service. It carries ZrO₂ minimum 28%, bulk density minimum 2.9 g/cm³, normal temperature compressive strength minimum 50 MPa after 110 °C drying, refractoriness minimum 1,770 °C, maximum service temperature 1,650 °C and use density 3,000 kg/m³. It is composed of molten corundum aggregate particles with a small amount of additives, so it has strong fluidity and is easy to ram, hardens at room temperature, holds high compressive strength at temperature, shows small thermal expansion and shrinkage and resists solution corrosion.

Q13. The zircon ramming mass datasheet shows ZrO₂ minimum 3.0%. Is that grade really good enough against molten glass?

That figure belongs to a natural zircon sand product, not a fused zirconia corundum grade, so do not compare it with the AZS ZrO₂ headline. The zircon grade uses natural selected zircon (ZrSiO₄) sand aggregate and powder with aluminum phosphate as binder, giving the best ratio of thermal conductivity and thermal shock resistance, with excellent inertness to molten glass and chemical slags. That is why it is the bottom-layer material for glass furnace bottom paving and anti-seepage. Values: bulk density minimum 3.5 g/cm³, compressive strength minimum 45 MPa, refractoriness minimum 1,790 °C, maximum service temperature 1,650 °C. For higher zirconia content, use fused AZS ramming mass, ZrO₂ minimum 28%.

Q14. When should I install a plastic instead of a ramming mass or a castable?

When the shape is irregular, or the duty is impact. Corundum-mullite plastic is kneaded like mud and hardens like steel, combining the extremely high refractoriness of corundum with the excellent thermal shock resistance of mullite; pneumatically rammed it fits any irregular complex furnace shape, such as around burner blocks and dead corners of furnace door frames, and forms a seamless solid lining after high temperature baking. High-strength wear-resistant plastic introduces extremely high-hardness corundum or silicon carbide particles for particle impact areas such as CFB boiler cyclone target zones, burner pipes and pulverized coal pipes.

Q15. My datasheet lists bulk density in g/cm³ and use density in kg/m³. How should I use both?

Check both against the same product before you compare two options. Fused AZS ramming mass is supplied at bulk density minimum 2.9 g/cm³ with a use density of 3,000 kg/m³. Zircon ramming mass is supplied at bulk density minimum 3.5 g/cm³ with a use density of 3,600 kg/m³. The fused AZS hot repair material is specified with a use density of 3,200 kg/m³. Note the conversion: 3,000 kg/m³ is 3.0 g/cm³, so the two figures are not one number written twice, and a datasheet that shows only one of them gives you half the picture.

Refractory Ball and Insulating Products

Q16. Which refractory ball grade should I use in a regenerator or a checker chamber?

Ten grades are available, grouped by chemistry. The alumina-rich options are the Mechanism High-Density High-Alumina Ball and the Mechanism High-Strength High-Density Aluminum Ball with alumina content of 75% or higher, and they reach a maximum service temperature of 1,900 °C. The magnesium-aluminum series, the Mechanism High-Strength Magnesium Aluminum Ball and the Mechanism Magnesium Aluminum Chrome Ball, carry magnesium content from 8.5 to 55 percent. The magnesium chromite series reaches magnesium content up to 85 percent. Across all ten grades refractoriness is 1,790 °C, apparent porosity is 18 to 23% and bulk density is 2.2 to 2.85 g/cm³.

Q17. Can bubble alumina be used as the aggregate in my own lightweight insulating castable?

Yes, it is supplied for that route, and also for lightweight insulating brick, high temperature furnace back-up lining and petrochemical reformer insulation. Two grades are offered. The High purity grade has Al₂O₃ minimum 99%, SiO₂ maximum 0.2%, Fe₂O₃ maximum 0.1% and Na₂O maximum 0.3%. The High strength grade has Al₂O₃ minimum 98.5%, SiO₂ maximum 1%, Fe₂O₃ maximum 0.08% and Na₂O maximum 0.25%. Both deliver stacking density 0.4-1 g/cm³, rate of reduction maximum 15% and a 0-7 mm particle size, with maximum working temperature 1,825 °C.

Q18. Bubble alumina brick or alumina hollow sphere product - which insulating brick should I specify?

They are different products, so decide on service temperature first. Bubble alumina brick is the shaped brick in four grades: CHSAH99 at Al₂O₃ minimum 99.3%, CHAH99 at 99%, CHAH90 at 90% and CHAH85 at 85%. Bulk density is 1.4-1.9 g/cm³, cold crushing strength minimum 12-18 MPa, initial softening temperature under load minimum 1,700 °C, thermal conductivity 0.55-0.75 W/(m·K) and maximum service temperature 1,750-1,800 °C. The alumina hollow sphere family runs higher, maximum service temperature 1,650-2,200 °C depending on grade, including a Sialon grade with ZrO₂ minimum 9.8%.

Q19. Which ceramic fibre module grade gives me the service temperature I need behind the hot face?

Five grades cover the range. CH-XWK40 has Al₂O₃ 40-44%, CH-XWK45 has 44-46%, CH-XWK48 has 46-50%, CH-XWK50 is a high alumina material with Al₂O₃ 50-60%, and CH-XWKZ15 is a zirconia contained material with Al₂O₃ 30-35% and ZrO₂ minimum 15%. Service temperature is maximum 1,000 to 1,350 °C depending on grade, volume density is 150-250 kg/m³ for all five, heating shrinkage is maximum 1.5% after 900-1,300 °C drying for 24 hours, and Al₂O₃+SiO₂ is minimum 94-97%. Modules sit in the standard petrochemical insulation matrix, alongside high alumina bricks, special fire clay bricks and lightweight insulation bricks.

Q20. When do I need ceramic fibre shaped pieces instead of modules?

When the detail is small, shaped and specific: observation holes, temperature measure holes, pressure measure holes, burner blocks, furnace doors, electric heating wire supporters, hot pipe lining, and molten aluminum collectors and grooves. These are made from refractory fibre by vacuum molding, with special moulds designed and produced to the shape and dimension you need, so the size is custom rather than standard. Five XWJ grades mirror the module chemistry, from CH-XWJ40 at Al₂O₃ 40-44% to the zirconia grade at Al₂O₃ 30-35% and ZrO₂ minimum 15%. Volume density is 200-600 kg/m³ and cold crushing strength minimum 0.2 MPa.

Q21. My furnace sees acid vapour rather than glass melt. Which brick and castable do I specify?

Acid-resistant brick is the shaped product for acid regeneration process furnaces and other acid-corrosion furnace service in power and petrochemical plants. Three NSZ grades are offered by bulk density: CH-NSZ1.0 at maximum 1.0 g/cm³, CH-NSZ1.3 at maximum 1.3 g/cm³ and CH-NSZ1.8 at maximum 1.8 g/cm³. Water absorption is maximum 12 to 15%, cold crushing strength minimum 10 to 20 MPa, acid proof minimum 96% and heating line change maximum 0.1% at 300 °C. For castable work in sulfuric acid and hydrochloric acid service, an acid-resistant castable uses special water glass or other acid-resistant chemical binders.

Hot Repair of Fused AZS

Q22. Which hot repair material do I use on damaged fused AZS brick?

Fused AZS hot repair refractory material, formulated for heat repair of glass melting furnace fused zirconia corundum bricks and aluminum masonry structures. It carries Al₂O₃ minimum 46%, ZrO₂ minimum 28% and SiO₂ maximum 20%, with 0.2MPa refractoriness under load of 1,610 °C and refractoriness minimum 1,790 °C. Cold crushing strength is minimum 30 MPa after 110 °C drying for 24 hours and minimum 35 MPa after 1,450 °C firing for 3 hours, and use density is 3,200 kg/m³. The structure is compact and low in porosity, with high temperature volume stability, strong bonding ability and convenient construction.

Q23. How do I patch damaged silica masonry without cracking it from quartz expansion?

Use special silicon patching refractory material, engineered for heat repair of glass kiln, coke oven and blast furnace hot blast stove silica masonry, and it will not damage the repaired structure through expansion of quartz. Refractoriness is minimum 1,750 °C and 0.2MPa refractoriness under load is minimum 1,700 °C. Cold crushing strength is minimum 30 MPa after 110 °C drying for 24 hours and minimum 35 MPa after 1,450 °C firing for 3 hours, permanent linear change is maximum 0.2% after that firing, apparent porosity is maximum 22% and use density is 2,300 kg/m³.

Q24. Which repair material goes where - AZS brick, silica masonry, or the kiln bottom structure?

Match the material to the masonry you are repairing. Fused AZS hot repair refractory material is for heat repair of glass melting furnace fused zirconia corundum bricks and aluminum masonry structures, with compact structure, low porosity, high temperature volume stability and strong bonding ability. Special silicon patching refractory material is for silica masonry in glass kilns, coke ovens and blast furnace hot blast stoves, with a high load-softening point, low temperature creep rate, and resistance to slag and erosion. For the kiln bottom structure itself, use zirconium corundum castable for cold patching and heat patching.

Q25. Can I cold-patch and hot-patch the glass kiln bottom safety layer and wall protective layer?

Yes, that is what zirconium corundum castable is for: cold patching and heat patching for the safety layer, the kiln wall protective layer and the upper structure of the glass kiln bottom. Three AZS grades are offered, each with Al₂O₃ minimum 45%. AZS50V carries ZrO₂ minimum 29% for the bottom sealing layer on the insulation layer, AZS60L carries ZrO₂ minimum 30% for the next layer of 50V bricks above, and AZS04J carries ZrO₂ minimum 30% for filling gaps between surface bricks. Resistance to glass erosion is good on all three and bubble precipitation tendency is weak.

Q26. Which alumina powder grade should I specify as filler or additive in a repair mix I compound myself?

Four grades are supplied. NX-1 has Al₂O₃ minimum 99.7% for high-purity industrial application, NX-2 minimum 99.5% for high-purity industrial application, NX-3 minimum 99.0% for general industrial application, and HX-1 minimum 99.5% for general industrial application. Na₂O is up to 0.10-0.20%, SiO₂ up to 0.05-0.15% and Fe₂O₃ up to 0.03-0.04% depending on grade, with true specific gravity minimum 3.93-3.95 g/cm³, alpha-Al₂O₃ minimum 94-95% and primary crystal size 1-4 micrometer. It is used in refractory castables, plastics, repair mixes, gunning mixes, coating mixes, binders and high-purity refractory fibres.

Q27. What do you need from me to prepare a hot repair material proposal, and what support comes with it?

For a repair, send the glass melting furnace drawing, the lining design, the kiln capacity and the operating temperature data, and add the damaged area, the repair specification and whether the work is hot or cold. The engineering team in Xinmi City, Zhengzhou, Henan, China then adjusts Al₂O₃, ZrO₂ and SiO₂ content, raw material formulation and the ceramic binder system against your service temperature and erosion conditions, and returns a tailored formulation proposal with optimized grade selection, raw material adjustment and the installation procedure. The consultation and on-site technical support are free.

Glass Furnace Engineering and Service

Q28. What does the float process as a whole demand from the refractory?

A float furnace is unforgiving: a single impurity drop destroys the entire glass sheet, so the refractories must be absolutely pure and extremely long-lived. The regenerative arrangement, today's mainstream, puts two huge independent regenerators full of checker refractory bricks beside the kiln, where combustion temperatures easily exceed 1,600 °C; the recuperative arrangement uses built-in metal or special ceramic heat exchangers and is not suitable for ultra-large float lines. The top arch takes extremely pure high-quality silica brick to avoid high-temperature collapse. The ultra-long pool wall containing the rolling hot glass lake is protected by dense fused AZS blocks. That whole top system escorts continuous operation at 1,500 °C, with an overhaul limit cycle of 8-12 years.

Q29. Why is the throat lined in AZS 41# while the regenerator above it is lined in alkaline brick?

Because the two zones fail in completely different ways. The regenerator carries a huge temperature difference along its height, so its configuration is stepped: the upper high-temperature zone suffers severe alkali fly ash corrosion and takes high-quality alkaline bricks, that is high-purity magnesia bricks and forsterite bricks; the middle zone uses spalling-resistant high alumina bricks or direct-bonded magnesia-chrome bricks; the lower low-temperature zone uses high-quality low-porosity fire clay bricks; and the checkerwork itself uses alkaline special-shaped bricks with extremely strong heat exchange capacity. The throat and flow hole see fast-moving glass, so they are built with the most erosion-resistant fused cast AZS blocks, especially AZS 41# with ZrO₂ content up to 44%.

Q30. What changes if my glass furnace burns alternative fuel such as waste glass and biomass?

The atmosphere and the refractory both get harder. To cut carbon emissions and fuel cost, glass plants mix waste glass and biomass into the fuel, and the consequences are severe: the originally stable kiln atmosphere becomes extremely oxidizing or extremely reducing, combustion temperature fluctuates wildly and frequent severe thermal shock spalling occurs. The furnace gas is filled with highly corrosive alkali salt vapour, with potassium, sodium and chlorine, which penetrates and dissolves the traditional refractory network structure. The response is a move to grades with higher alkali penetration resistance and stronger thermal shock resistance.

Q31. Can the same AZS products be used outside glass, and what service life do you commit to?

Yes, on nonferrous smelting duty the same chemistry is used in a different combination. For nonferrous smelting shaft furnaces, sulfur combustion furnaces and alkali sulfide converters, the package is built on customized 3D fluid analysis and low-NOx burner design, and the core materials are highly chemical-resistant AZS ramming mass, fused zirconia corundum blocks and direct-bonded magnesia-chrome bricks, combined with Solidworks and Fluent CFD simulation for the brick layout. The service life commitment for nonferrous smelting furnaces in highly corrosive environments is more than 8 years, and AZS ramming mass plus hot repair technical support continues after commissioning.

Q32. Which refractory families do you specify for the nonferrous and chemical furnaces my company also runs?

Each process attacks the lining differently. Copper smelting, whether modern flash smelting or the traditional reverberatory furnace, produces highly corrosive acidic iron copper silicate slag, so only high-strength fired magnesia-chrome bricks and direct-bonded magnesia-chrome bricks hold the line. Nickel-iron smelting reduces laterite in a rotary kiln at 1,200-1,400 °C and melts it in an electric furnace, so the kiln lining takes magnesia-alumina and magnesia-chrome wear-resistant castables. Lead-zinc smelting roasts at 1,000-1,300 °C under strong acidic SO₂ flue gas and alkali vapour, so the line needs anti-sulfuric acid gas penetration castables and anti-corrosion special bricks.

Q33. When do you use chrome corundum brick instead of magnesia-chrome brick?

Chrome corundum brick is made by mixing high-purity alumina with chromium oxide (Cr₂O₃) and firing at high temperature, and the chromium oxide is what gives it both the extremely high strength and the corrosion resistance that can hardly be penetrated or dissolved. It is the answer where the environment is coal chemical water-coal slurry gasifiers, carbon black reactors, and refining environments with severe strong acid and alkaline slag erosion. Magnesia-chrome brick, including the direct-bonded version, remains the standard for copper smelting, where the acidic iron copper silicate slag is the dominant attack.

Q34. What do you need from me to turn this into a lining proposal for my glass furnace?

Four things, and the more of them you have, the sharper the proposal. The glass furnace or glass kiln drawing, the lining design, the kiln capacity, and the operating temperature data. From those, our engineering team in Xinmi City, Zhengzhou, Henan, China adjusts ZrO₂, SiO₂, Na₂O, Fe₂O₃+TiO₂ and the combined alkali-and-oxide content against your service temperature and erosion conditions, and selects the casting type, PT-QX, ZWS or WS. You get a free consultation, on-site technical support, and a tailored formulation proposal with grade selection and raw material adjustment.

Industry Knowledge for Refractory Buyers

How do I select between AZS 33, 36 and 41 grade blocks?

The core is the zirconia purity of the fused cast block. AZS 33 with 32 to 36 percent ZrO2 balances corrosion resistance and cost and is laid in pool wall areas and upper structural layers that do not contact the glass. AZS 36 with 35 to 40 percent ZrO2 guards the pool bottom, corners and the more exposed positions. AZS 41 with 40 to 44 percent ZrO2 is the highest grade and is fixed at the charging port crown and throat where corrosion is worst.

What does the static corrosion rate of molten glass actually mean?

It is the millimetre of glass consumed per 24 hours from a test coupon held in static contact with normal soda-lime glass at 1,500 °C for 36 hours. AZS 33 holds at maximum 1.50 mm per 24 hours, AZS 36 at 1.40 mm and AZS 41 at 1.30 mm. Lower numbers mean longer life at the glass contact surface, and the difference between grades matters most where the coupon is directly immersed.

Why does the glass furnace crown require silica brick specifically?

The crown spans a large opening above 1,500 °C and must resist alkali vapour corrosion while allowing no impurity to fall into the glass. High quality silica brick with SiO2 above 95 percent has almost no residual expansion above 300 °C, extremely high refractoriness under load, and a safe life usually reaching 8 to 12 years. Its main weakness is poor thermal shock performance, so the crown bake curve must be controlled through the quartz transformation point.

How is a glass furnace regenerator lined, and what governs the checker material?

The regenerator carries a very large temperature difference from top to bottom, so the material configuration is stepped by zone. The hot upper zone takes high-quality alkaline brick such as high-purity magnesia or forsterite against severe alkali and dust corrosion. The middle zone uses spalling-resistant high alumina or direct-bonded magnesia-chrome brick. The cooler lower zone takes high-quality low-porosity fire clay brick. The checkerwork itself uses alkaline special-shaped brick with strong heat exchange capacity.

What is the difference between a regenerative and a recuperative glass furnace?

The regenerative type is today's dominant mainstream. Two large independent regenerators filled with checker brick stand beside the furnace and periodically switch exhaust gas and cold air channels, recovering very high temperature heat to preheat the incoming air, giving very high combustion efficiency with temperatures readily above 1,600 °C. The recuperative type uses built-in metal or special ceramic heat exchangers so the exhaust gas continuously transfers heat through the tube wall, which is simple and compact but not suitable for very large float lines.

How do I select refractory for the glass furnace throat and flow hole?

The throat and flow hole connect the melting zone to the cooling zone, and the glass flows through them at speed, so erosion there is the most severe in the whole furnace. It must be built with the most erosion-resistant fused cast AZS blocks, particularly AZS 41 with ZrO2 content up to 44 percent, for the surrounding masonry. This is the single most corrosion-critical position in a glass furnace.

Why do bubbles precipitate from the refractory into the glass?

Gas trapped in the pores of a lining migrates into the molten glass and forms bubbles, which is why the bubble precipitation rate is one of the specified quality parameters for AZS blocks. The grades measure 2.0 percent at 1,300 °C for 10 hours for AZS 33, 1.5 percent for AZS 36 and 1.0 percent for AZS 41. Weak bubble precipitation tendency is the property that protects the glass quality.

What is the role of refractory balls in a glass furnace regenerator?

Refractory balls are the heat storage medium in ball-type regenerators, made mainly from alumina based material by pressing and sintering. They are used together with checker brick and rely on their very large specific surface area to preheat the gas flow rapidly and store the heat. Alumina content grades run from 60 to 95 percent with diameters usually between 20 and 50 mm.

Nonferrous Casting Refractory: Copper, Nickel, Zinc and Lead Smelting

Questions: 35

Questions in this section
  1. Copper and Nickel Smelting Furnaces (4)
  2. Lead-Zinc Smelting and Zinc Volatilisation (4)
  3. Direct Bonded Magnesia-Chrome and Spinel (4)
  4. Anti-Seepage and Cathode Protection (4)
  5. Rotary Kiln and Auxiliary Equipment Materials (6)
  6. Nonferrous Plant Engineering and Service (6)
  7. Industry Knowledge for Refractory Buyers (7)

Copper and Nickel Smelting Furnaces

Q1. Which lining survives the acidic iron copper silicate slag in a copper smelter?

Copper smelting produces a highly corrosive acidic iron copper silicate slag, and that slag decides the lining. Two routes are proven. The traditional reverberatory furnace relies on sidewall burners with long flames to bake and reflect the smelt. Modern overlord flash smelting occupies more than half of the global refined copper production: concentrate powder is mixed with oxygen-enriched air and sprayed into the furnace chamber at explosive speed, where it instantly oxidises and melts in the air and releases massive heat. In both environments only high-strength fired magnesia-chrome bricks and the more expensive direct bonded magnesia-chrome bricks can become the key armour holding the defence line.

Q2. We run flash smelting instead of a reverberatory furnace. Does that change the lining?

It changes the duty, not the lining principle. The traditional reverberatory furnace relies on sidewall burners with long flames to bake and reflect the smelt. Modern overlord flash smelting occupies more than half of the global refined copper production, where concentrate powder mixed with oxygen-enriched air is sprayed into the furnace chamber at explosive speed, instantly oxidises and melts in the air and releases massive heat, so it is extremely efficient and low-consumption. Both routes produce the same highly corrosive acidic iron copper silicate slag, so what decides the lining is where that slag runs and how hot each zone gets.

Q3. Our nickel-iron rotary kiln lining keeps getting rubbed and eroded. What do you specify?

Nickel-iron production is hard on a rotary kiln. A huge and long kiln takes wet laterite ore to reduce, dehydrate and pre-roast it at 1,200-1,400 °C, and laterite impurities are so complex that the kiln lining is severely rubbed and eroded. The red-hot ore then rushes into a giant electric furnace that melts it with tens of thousands of amperes of arc. The answer is a heavy-duty wear-resistant and spalling-resistant premium magnesia-alumina and magnesia-chrome high-strength wear-resistant castable, with the reduced nickel kiln grades CH-HZ45 and CH-HZ55 carrying the preheating zone and reduction zone at Al₂O₃ minimum 45% and 55% with Fe₂O₃ maximum 1.2%.

Q4. Which refractories go into an RH vacuum degasser vessel and its circulation tubes?

The RH unit runs extreme degassing and decarburisation. The vacuum vessel and the circulation tubes withstand extreme vacuum and high-speed circulating washing of molten steel, and mainly use high-quality direct bonded or semi-direct bonded MgO-Cr₂O₃ magnesia-chrome bricks. The lower vessel often uses a high-strength spinel castable, the immersion tube area uses special immersion fired bricks, and the vacuum pipeline is supplemented with special protective coatings. The same magnesia-chrome family is specified for copper and nickel smelting, so a plant running both can hold one specification and one inspection regime instead of two.

Lead-Zinc Smelting and Zinc Volatilisation

Q5. What does the lead-zinc process actually do to a refractory lining?

It doubles the corrosion load. Highly toxic sulfur-containing lead-zinc concentrate is charged into a fluidised bed roasting furnace or a rotary kiln, where sulfides are forcibly oxidised to crude oxides at 1,000-1,300 °C while discharging large amounts of high-concentration sulfur dioxide toxic gas. The material is then sent for agglomeration sintering, and finally charged with coke into a closed blast furnace or an imperial smelting furnace, the ISP method, for reduction and melting into metal primary liquid. The entire line sits in extremely strong concentrated sulfur dioxide acidic flue gas plus high-concentration alkali vapour, and very few materials survive that combination.

Q6. What protects the lead-zinc line from sulfur dioxide and alkali vapour?

The whole line must carry specially developed advanced castables that resist sulphuric acid gas penetration, plus anti-corrosion special bricks, because the entire process is filled with extremely strong concentrated sulfur dioxide acidic flue gas and high-concentration alkali vapour double poisoning corrosion, and very few materials can survive it. Our castables for zinc, nickel and lead smelting rotary kiln come as five JZ grades for the same duty, with strong acid and alkali corrosion resistance and good wear resistance. Send the rotary kiln drawing, lining layout, capacity and operating temperature data, and the grade, binder system and installation procedure are set against your conditions.

Q7. Which castable grade for a zinc, nickel or lead smelting rotary kiln?

Five JZ grades cover the duty: CH-JZ55 at Al₂O₃ minimum 55% for general demand, CH-JZ60 at minimum 65% for higher demand, CH-JZ75 at minimum 75% for high demand, CH-JZ80 at minimum 80% for higher demand, and CH-JZ85 at minimum 85% for the highest demand. Across the range bulk density is minimum 2.3 to 2.8 g/cm³, modulus of rupture minimum 8 to 12 MPa, cold crushing strength minimum 50 to 100 MPa, and thermal shock resistance minimum 30 cycles at 900 °C water cooling for all five grades, with maximum service temperature 1300 to 1600 °C depending on grade. Grade on service temperature first, then on erosion rate.

Q8. Which brick belongs in a zinc volatilisation kiln, and can it be tailored to our furnace?

The magnesia-alumina-chrome spinel composite brick, made by high-pressure moulding and high-temperature sintering from high-purity magnesia and magnesia-chromium composite spinel as the main raw materials. MAGE-75A is MgO minimum 75%, Al₂O₃ 9-13% and Cr₂O₃ maximum 3-6% for the highest-demand service; MAGE-75B is MgO minimum 70% with the same Al₂O₃ 9-13% and Cr₂O₃ maximum 3-6% for higher demand. Chemistry, grade and geometry are optimised against your specific zinc volatilisation kiln, copper smelting furnace or other erosion-serious parts design and operating conditions, so send the furnace drawing, lining layout, kiln capacity and operating temperature data and you get a free consultation, on-site technical support and a tailored proposal.

Direct Bonded Magnesia-Chrome and Spinel

Q9. How do I choose between the eight CHZMGe direct bonded magnesia-chrome grades?

The grade code carries the chemistry. CHZMGe 20A is MgO minimum 45% with Cr₂O₃ minimum 30%, and 20B is MgO minimum 40% with Cr₂O₃ minimum 30% for high-chrome nonferrous smelting service. Then 18A at 50% MgO and 26% Cr₂O₃, 18B at 45% and 26%, 16A at 52% and 24%, 16B at 47% and 24%, 14A at 60% MgO and 20% Cr₂O₃, and 14B at 55% and 20%. Across all eight grades bulk density is minimum 3.20 to 3.38 g/cm³, apparent porosity maximum 15% to 16%, cold crushing strength minimum 50 MPa, and 0.2MPa refractoriness under load minimum 1700 °C.

Q10. Which zones of a copper or nickel smelting furnace wear out first, and what goes there?

The erosion-serious parts, and the direct bonded magnesia-chrome family is built for exactly those locations: circulation tubes, bottom grooves, the dipping tube, the bottom through, the central through and the upper through. The brick family carries good high temperature resistance and peeling resistance, which is what you need in the places where temperature fluctuations are large and high. Grade those zones highest and step the rest down. Send the furnace drawing, lining layout, capacity and operating temperature data and our engineers in Xinmi City, Zhengzhou will tune MgO, Cr₂O₃, Fe₂O₃ and SiO₂ content, raw material formulation and the sintering process to your service temperature and erosion conditions.

Q11. Is direct bonded magnesia-chrome brick worth the extra cost over fired magnesia-chrome brick?

In the zones that decide the campaign, yes, because the price difference is a service-life difference. In the harshest copper smelting environments only high-strength fired magnesia-chrome bricks and the more expensive direct bonded magnesia-chrome bricks can become the key armour holding the defence line. The direct bonded route uses high-purity magnesia and imported chrome concentrate with a small amount of additives, made under high pressure and high temperature, and it brings good high temperature resistance and peeling resistance, which is what you need in locations where temperature fluctuations are large and high.

Q12. Can the direct bonded grade be customised to our furnace design and operating conditions?

Yes, and that is where the real value is. Custom chemistry, grade and geometry optimisation is done against your specific copper or nickel smelting furnace design and operating conditions, with the engineers adjusting MgO content, Cr₂O₃ content, Fe₂O₃ content, SiO₂ content, raw material formulation and the sintering process to meet your service temperature and erosion conditions. Send the furnace drawing, lining design, furnace capacity and operating temperature data to our engineering team in Xinmi City, Zhengzhou, Henan, and you get a free consultation, on-site technical support and a tailored proposal with optimised grade selection, raw material adjustment and geometry design.

Anti-Seepage and Cathode Protection

Q13. What is anti-seepage castable and where does it go in a nonferrous plant?

Anti-seepage castable is supplied as the CH-TLD grade with Al₂O₃ content maximum 35%, developed for nonferrous metal electrolytic cell and rotary kiln service. On a rotary kiln it covers the kiln mouth, the pre-tropical zone, the calcination zone, the cooling machine and the feed nozzle, and it suits the calcination and roasting of cement, limestone, magnesia, ilmenite and non-ferrous metal ore. The family gives high strength, high wear resistance, anti-flaking and anti-scouring, with strong acid and alkali corrosion resistance and long service life. Bulk density is minimum 2.1 g/cm³ after 110 °C curing for 24 hours.

Q14. How does anti-seepage castable actually stop electrolyte penetrating the lining?

Chemically, at the hot face. The material reacts with the electrolyte alkali metal ions at high temperature to form a glaze layer on its surface, and that glaze layer prevents penetration of the glass phase in the raw material. That is what produces the anti-skinning effect: the surface stays sealed instead of fusing and running. The mechanical backing is conventional, with cold crushing strength minimum 50 MPa after 110 °C curing for 24 hours and minimum 60 MPa after 1000 °C firing for 3 hours, modulus of rupture minimum 8 MPa and 10 MPa, and thermal conductivity maximum 0.5 W/m·K at 350 °C and 0.7 W/m·K at 650 °C.

Q15. What is the dry anti-seepage material and what does it protect?

It protects the cathode block of a nonferrous metal electrolytic cell, the aluminium electrolysis case. The dry anti-seepage material is supplied as the TSL grade with Al₂O₃ content maximum 40%, and has simple construction, good thermal insulation effect and strong anti-permeability. It reacts with alkali ions in the materials and metal liquids at high temperature and forms an isolation layer on the surface, so sodium salt cannot infiltrate into the cathode block, which prolongs the service life of the electrolytic cell and reduces power consumption. Tamp volume weight 1.9±0.1 g/cm³, refractoriness minimum 1600 °C, thermal conductivity maximum 0.35 W/m·K at 350 °C and 0.43 W/m·K at 650 °C.

Q16. For the cell, do we use the castable or the dry material?

Both, on different sides of the problem. The dry anti-seepage material goes where the cathode block needs protection from alkali ions in the materials and metal liquids, because the isolation layer stops sodium salt infiltration, the good thermal insulation effect cuts heat loss, and the result is a longer service life for the electrolytic cell and lower power consumption. The CH-TLD anti-seepage castable goes on the cell and rotary kiln lining where wear, flaking and scouring drive failure, and it is the stronger option. Send the cell drawing, cathode block design, cell capacity and operating temperature, and the grade and installation procedure are set for your service conditions.

Rotary Kiln and Auxiliary Equipment Materials

Q17. What goes in the preheating zone and the reduction zone of a reduced nickel kiln?

Two grades matched to two zones, both built on low iron mullite and flint clay as the main raw materials. CH-HZ45 is Al₂O₃ minimum 45% with Fe₂O₃ maximum 1.2% for general reduced nickel kiln preheating zone service, and CH-HZ55 is Al₂O₃ minimum 55% with Fe₂O₃ maximum 1.2% for the higher-demand reduction zone. The low cement system gives excellent CO erosion resistance, high strength and good thermal shock resistance. Bulk density is minimum 2.3 to 2.4 g/cm³ after 110 °C drying for 24 hours, cold crushing strength minimum 45 to 60 MPa, thermal conductivity maximum 1.0 to 1.1 W/m·K at 800 °C hot side, maximum service temperature 1100 to 1400 °C.

Q18. Which castable for a carbon baking furnace and the nonferrous rotary kiln zones around it?

The carbon baking furnace and nonferrous rotary kiln range covers the kiln mouth, the pre-tropical zone, the calcination zone, the cooling machine and the feed nozzle. Five grades: CH-TLD and CH-TLQ general service, CH-TLZ45 at Al₂O₃ minimum 45% at 1400 °C, CH-TLZ60 at minimum 60% at 1450 °C, and CH-TLZ70 at minimum 70% at 1500 °C maximum service temperature. Bulk density is minimum 2.2 to 2.5 g/cm³ after 110 °C curing for 24 hours, modulus of rupture minimum 6 to 8 MPa, cold crushing strength minimum 30 to 50 MPa, permanent linear change ±0.1 percent after 110 °C curing and ±0.4 percent after 1000 °C firing for 3 hours.

Q19. Which mortar and spray coating for joints, pipelines and flues?

They solve different problems, so they are specified separately. Seven refractory mortar grades are available: CH-GA88 at alumina minimum 88% for high-alumina brick masonry joints, CH-GACr88 at Cr₂O₃+Al₂O₃ minimum 88% for corundum-chrome brick joints, CH-GM85 at MgO+Al₂O₃ minimum 85% for magnesia-alumina brick, CH-GMCr85 for chrome-enhanced performance, and CH-GT85, CH-GT80 and CH-GT70 at 85%, 80% and 70% alumina. Refractoriness is minimum 1500 to 1690 °C, hardening time 60 to 180 seconds, adhesive strength minimum 1 MPa. For pipelines and flues, CH-PTL40 and CH-PTL45 spray coating come in light, medium or heavy grades, bulk density minimum 1.0 to 1.95 g/cm³.

Q20. What do you use for the furnace roof, the burner block connection and the partition?

Three structural families, each carrying a different load. Anchor brick is used at the furnace roof and in the suspended lining, produced from the same material as the lining castables: CH-MG48 and CH-MG55 at Al₂O₃ minimum 48% and 55%, refractoriness minimum 1730 to 1750 °C, bulk density minimum 2.30 to 2.35 g/cm³, apparent porosity maximum 21% to 22%, cold crushing strength minimum 45 to 50 MPa, permanent linear change maximum 0.5 percent after 1400 °C firing for 3 hours. Frame brick CH-BK55, CH-BK60 and CH-BK65 handles the lining frame and burner block connection, and hanger brick CH-DG1.8 and CH-DG2.0 the charge gate, discharge gate and annular heating furnace partition.

Q21. Which refractory goes in the cooler zones and the backup lining behind the working layer?

High alumina brick takes the hotter backup, in four LZ grades: CH-LZ75 at Al₂O₃ minimum 75%, CH-LZ65 at 65%, CH-LZ55 at 55% and CH-LZ48 at 48%. Cold crushing strength is minimum 40 to 54 MPa, apparent porosity maximum 22% to 23%, load softening temperature minimum 1420 to 1520 °C and refractoriness minimum 1750 to 1790 °C. Fire clay brick grades N-1 down to N-6 take the colder zones and insulation, at refractoriness minimum 1580 to 1750 °C, load softening temperature minimum 1300 to 1400 °C at 0.2 MPa, apparent porosity maximum 22% to 28%, cold crushing strength minimum 15 to 30 MPa.

Q22. Where do silica brick, acid-resistant brick and plastic refractory fit in the plant?

Common silica brick is the dense acid refractory for cooler, slag-free zones such as industrial furnace, coke oven and hot blast stove combustion chamber lining, in CH-GZ95, CH-GZ94 and GZ-93 grades at silica content 95%, 94% and 93%, refractoriness 1710, 1710 and 1690 °C, cold crushing strength 29.4, 24.5 and 19.6 MPa, and load softening start temperature 1620 to 1670 °C. Acid-resistant brick CH-NSZ1.0, CH-NSZ1.3 and CH-NSZ1.8 is for acid regeneration process furnace lining, with acid proof minimum 96 percent and water absorption maximum 12% to 15%. Plastic refractory CH-blS50, at Al₂O₃ minimum 50%, lines furnace roof, wall and fume pipe.

Nonferrous Plant Engineering and Service

Q23. Which insulating and heat storage materials do you supply for the plant?

Alumina hollow sphere products are used for kiln working lining and thermal insulation, in CH-KXQ88 at Al₂O₃ minimum 88%, CH-KXQ98 at minimum 99%, and the CH-KXQ98 Sialon grade with ZrO₂ minimum 9.8%. Bulk density is 1.30 to 3.0 g/cm³, cold crushing strength minimum 8 to 15 MPa, load softening temperature minimum 1650 to 1700 °C at 0.2 MPa, thermal conductivity maximum 0.5 to 1.0 W/m·K at 800 °C, maximum service temperature 1650 to 2200 °C. For regenerator heat storage, refractory balls come in ten grades with refractoriness 1790 °C across all grades and maximum service temperature reaching 1900 °C for the alumina-rich grades.

Q24. Can we buy the raw materials and make our own bricks and castables?

Yes. Refractory grade bauxite comes in five grades, RK70 through RK87, with Al₂O₃ minimum 70% to 87%, Fe₂O₃ maximum 1.5% to 2%, TiO₂ maximum 4 percent for the RK80, RK85 and RK87 grades, CaO+MgO maximum 0.4% to 0.6%, K₂O+Na₂O maximum 0.4% to 0.6%, bulk density 2.95 to 3.35 g/cm³ and water absorption maximum 3% to 5%, supplied as 0-0.3mm to 5-8mm aggregate and 100, 200 or 325 mesh powder. Alumina powder is supplied as NX-1, NX-2, NX-3 and HX-1 at Al₂O₃ minimum 99.0% to 99.7%, Na₂O up to 0.10% to 0.20%, true specific gravity minimum 3.93 to 3.95 g/cm³ and alpha-Al₂O₃ minimum 94% to 95%.

Q25. Which refractory cement do you specify as the castable binder?

Four grades, and the choice turns on Al₂O₃ level and setting behaviour. A600 is Al₂O₃ minimum 50% for general refractory castable binder service, A700 is 50% to 60% for higher demand, A900 is minimum 53.5% for high demand, and CA-70 is 68.5% to 70.5% for the highest demand, with CaO 28.5% to 30.5%. Specific surface is minimum 300 to 350 m²/kg, setting time initial minimum 45 to 180 minutes and final maximum 150 to 360 minutes, and cold crushing strength 24 hour minimum 40 to 72 MPa and 72 hour minimum 45 to 82 MPa. It is calcium aluminate cement, made from bauxite and limestone.

Q26. What does your engineering and hot repair service cover on site?

Zoning first, then grading. Our reference projects are the 200-300 ton ladle jobs, where the zoning is explicit: cost-optimized advanced MgO-C in the slag line, Al₂O₃-MgO-C or magnesia-chrome in the sidewall, low-carbon corundum-spinel in the molten steel impact zone to strengthen erosion resistance, and a safety layer insulating castable with conventional gunning mix behind it for hot repair. Solidworks 3D thermal modeling identifies the key wear areas and targeted grade upgrades reduce refractory cost and downtime by 30%, and red-hot gunning every 5-10 heats extends the overall service life by up to 30%. The same discipline applies to your nonferrous zoning.

Q27. Should we buy precast blocks and a furnace cap castable instead of casting on site?

For shaped, critical geometry, precast is usually the safer route. The working layer precast block is cast in a constant-temperature plant using precision moulds, high-frequency vibration, curing and strictly curve-controlled baking, then shipped as single pieces for direct lifting, which greatly saves on-site baking time and avoids construction hazards; impact pads, flow stabilizers and delta blocks are typical parts. The special castable for arc furnace cap and the large ladle furnace LF refining furnace triangle area is supplied as DLD75, DLD80, DLD90 and DLD92 at Al₂O₃ minimum 75% to 92%, with bulk density minimum 2.6 to 3.1 g/cm³ and compressive strength minimum 60 to 100 MPa.

Q28. What service life do you commit to, and what happens after commissioning?

The commitment is more than 8 years of service life for nonferrous smelting furnaces under highly corrosive environments. That figure only holds if the material supply and the repair support hold with it, so once the project is put into operation we keep supplying the AZS ramming mass and the maintenance technical support needed for hot repair, ensuring continuous production. Plan the hot repair route and the ramming material stock for the campaign rather than sourcing it after the furnace has stopped.

Industry Knowledge for Refractory Buyers

Why are copper smelting furnace linings attacked so severely?

Both extreme copper smelting processes produce highly corrosive acidic iron-copper silicate slags. The flash smelting route reacts copper concentrate with oxygen-enriched air at explosive speed, and the reverberatory furnace bakes and reflects melt with long sidewall flames. Only high-strength fired magnesia-chrome brick and the more expensive direct-bonded magnesia-chrome brick can hold the defence line in that environment, which is why direct-bonded grades dominate nonferrous service.

What is the difference between direct-bonded and fused magnesia-chrome brick?

Direct-bonded magnesia-chrome brick is made by high-temperature co-sintering high-purity periclase and chrome concentrate, so the two phases bond directly into a continuous network. That gives it the highest refractoriness under load at 0.2 MPa and the strongest resistance to alkaline slag, which is why it is specified for circulation tubes, bottom grooves, dipping tubes and bottom through positions in nonferrous smelting furnaces.

How is the lining of a zinc volatilisation kiln protected?

Zinc volatilisation kilns run a strongly alkaline, oxidising atmosphere in which the vapour phase attacks conventional linings. Direct-bonded magnesia-chrome brick and fused zirconia corundum blocks provide the primary armour, combined with highly chemical-resistant AZS ramming mass for the sealing and repair zones. Brick layout is refined against Solidworks and Fluent CFD simulation results.

How does cathode protection work in aluminium electrolysis cells?

In aluminium electrolysis the cathode block lining is attacked from the metal side and the electrolyte side, so protection is a designed system rather than a single material. Dry anti-seepage material reacts with alkali ions in the metal at high temperature to form an isolation layer on the surface, which blocks sodium salt infiltration into the cathode block and extends cell life while reducing power consumption. Carbon blocks remain the structural base beneath it.

What are the standard lining positions in a nickel-iron smelting furnace?

The nickel-iron process is long and rough on linings: wet laterite ore is first reduced and pre-roasted in a long rotary kiln at 1,200 to 1,400 °C, then the red-hot ore is charged into an electric furnace for melting. Because laterite impurities are extremely complex, the rotary kiln lining is worn and eroded hard, which is why heavy-duty wear-resistant and spalling-resistant magnesia-alumina and magnesia-chrome castables are specified there.

Why is chrome-magnesia brick being replaced in nonferrous service?

Traditional magnesia-chrome brick generates highly toxic and carcinogenic hexavalent chromium when used in high-temperature alkaline atmospheres, and major regulations now restrict waste landfill. Magnesia-alumina spinel brick has no chromium, no environmental liability, and with optimised formulation it reaches equivalent corrosion resistance and coating adhesion. For a new nonferrous project, chrome-free spinel is now the default choice.

What service life can be expected from a nonferrous smelting furnace lining?

For nonferrous smelting furnaces under highly corrosive environments, the company commits to a long-term service life of more than 8 years. That commitment is backed by the material selection, the 3D CFD fluid simulation driven layout and the ongoing hot repair material supply and technical support provided after commissioning.

Power and Petrochemical Refractory

Questions: 41

Questions in this section
  1. Ethylene Cracking and Reformer Furnaces (5)
  2. CFB Boiler Wear Linings (6)
  3. Acid Resistant and Chemical Service Materials (5)
  4. Ceramic Fibre Products and Insulation (5)
  5. Wear Resistant Castables and Plastics (6)
  6. Power and Petrochemical Project Service (7)
  7. Industry Knowledge for Refractory Buyers (7)

Ethylene Cracking and Reformer Furnaces

Q1. Which refractory goes in each layer of an ethylene cracking furnace lining?

Buy the layers separately, because they do different jobs. The outer layer is ceramic fiber blanket, at 95 to 160 kg/m³ and thermal conductivity maximum 0.14 to 0.28 W/m·K, or the compressed module form, to kill heat loss. The middle layer carries the gradient: insulating fire clay brick in grades NG-0.5 to NG-1.0, or lightweight insulating castable in grades CH-QJ0.5 to CH-QJ1.8. The hot face working layer takes the combustion gas flow erosion, so it is high-grade high alumina plastic or high-strength lightweight castable, with cold crushing strength minimum 50 to 95 MPa and normal wear maximum 8 to 10 cm³.

Q2. What life should I plan for each layer of an ethylene cracking furnace lining, and what extends it?

Depending on the operating environment and the maintenance level, the ultra-lightweight ceramic fiber modules in the inner working area of an ethylene cracking furnace usually last 3 to 6 years, while traditional brick or cast heavy-duty insulating linings last 5 to 10 years. Regular surface thermal anti-corrosion spraying extends that life further, because it keeps the exposed surface from degrading between shutdowns. Plan your replacement cycle around the module, not the brick, because the module is the part that is renewed first.

Q3. Which refractories do you actually use across a petrochemical plant?

Petrochemical service is not one material, it is a matrix covering four very different duties. High alumina bricks and special fire clay bricks do the masonry, various lightweight insulation bricks carry the heat, and ceramic fiber modules handle the furnace walls and roof. On top of that sit the high-performance special castables and high-temperature plastics, which are the products dedicated to ethylene cracking furnaces, reforming furnaces, hydrogen production converters and circulating fluidized bed boiler linings. A quotation that offers one product for all of it is mixing up the insulation duty and the erosion duty.

Q4. Which insulation suits a reformer, a hydrogen furnace or a carbon black reactor?

Bubble alumina brick is the workhorse for petrochemical methane reformer, hydrogen furnace and carbon black reactor lining. It is made from high-purity alumina fused and blown into hollow microspheres above 2100 °C, giving bulk density 1.4 to 1.9 g/cm³, cold crushing strength minimum 12 to 18 MPa, initial softening temperature under load minimum 1700 °C, thermal conductivity 0.55 to 0.75 W/(m·K) and maximum service temperature 1750 to 1800 °C. Four grades are offered: CHSAH99, CHAH99, CHAH90 and CHAH85. Bubble alumina itself, the hollow sphere aggregate with stacking density 0.4 to 1 g/cm³ and maximum working temperature 1825 °C, is what you blend into lightweight insulating castable and brick.

Q5. Our hydrogen unit runs at temperature with steam around it. How does that change the lining?

Hydrogen service changes the chemistry requirement, not the thickness. Under a hydrogen reduction atmosphere at 1,050 to 1,100 °C, high-temperature hydrogen strongly reduces and deoxygenates the iron oxide and silicon oxide components in traditional refractories, which causes structural disintegration, and the higher operating temperature limits what can be used at all. The third problem is steam: high-temperature steam generated by the hydrogen-oxygen reaction severely corrodes silicon-based materials. The solution is zero-iron, zero-silica high-purity magnesia-chrome brick, or alumina-magnesia spinel brick with an optimized pore structure, wherever hydrogen-based direct reduction meets electric arc furnace routes.

CFB Boiler Wear Linings

Q6. Which CFB boiler zones take the heaviest particle load, and what is used in each?

The CFB lining is heavy-duty anti-wear armor, developed to take the cyclic erosion of dense coal and desulfurization agent particles moving at extremely high speed. Three product types cover it: extremely high-density wear-resistant castables for the built lining, wear-resistant plastics where the geometry prevents casting, and gunning mixes dedicated to hot-state emergency repair. The zones that decide the campaign are the cyclones, the target areas and the return feeders, because that is where the particle load peaks and where the bed material repeatedly changes direction.

Q7. Which grade of wear-resistant castable belongs in the anti-wear lining?

Four corundum-mullite grades cover the CFB anti-wear lining: CH-MJZ70, CH-MJZ75, CH-MJZ80 and CH-MJZ85, carrying alumina minimum 70, 75, 80 and 85 percent with silica maximum 26, 21, 16 and 11 percent. Bulk density is minimum 2.7 to 2.9 g/cm³, cold crushing strength minimum 60 to 110 MPa, modulus of rupture minimum 8.5 to 16.0 MPa, and normal wear maximum 5 to 7.5 cm³. Refractoriness under load at 0.2 MPa is minimum 1450 to 1560 °C, thermal shock resistance is minimum 20 to 25 cycles at 900 °C water cooling, and maximum service temperature is 1550 to 1600 °C.

Q8. When do you use a refractory plastic instead of a castable in a CFB?

Use plastic where the geometry will not accept formwork casting, or where you need a repair without a long shutdown. High-strength wear-resistant refractory plastic, grades CH-KSL68, CH-KSL72 and CH-KSL75, is built from special-grade alumina, mullite, corundum and silicon carbide, mixed with binder, additive and plasticizer. It gives cold crushing strength minimum 50 to 95 MPa, normal wear maximum 8 to 10 cm³, thermal conductivity 1.5 W/m·K, thermal shock resistance minimum 30 cycles at 900 °C water cooling and a plasticity index of 15 to 40 percent. Dense ramming gives it metal-like resistance to grinding, which is why it is the repair material for cyclone target zones and pulverized coal pipes.

Q9. Corundum-mullite-SiC plastic or corundum-mullite plastic — which one?

Five grades are available and they split on the aggregate, so match the grade to the erosion severity. GMS-65, GMS-75 and GMS-85 are corundum-mullite based with alumina minimum 65, 75 and 85 percent, for general, higher-demand and highest-demand CFB service. TG-60 and TG-70 are silicon carbide based with SiC minimum 60 and 70 percent, for silicon carbide refractory plastic service in the worst particle streams. After 850 °C firing for 3 hours both families give cold crushing strength minimum 60 to 90 MPa and normal wear maximum 5 to 7 cm³, with permanent linear change 0.4 to 0.6 percent and thermal shock resistance minimum 25 to 40 cycles.

Q10. Where does a self-flowing castable earn its place?

Self-flowing castable is the answer where you cannot compact a conventional castable in a narrow or complex section, such as CFB boiler difficult construction locations. CH-ZLJZ75 and CH-ZLJZ80 give alumina minimum 75 and 80 percent with silica maximum 20 and 16 percent, and a self flow value of minimum 200 mm, so the material fills the form under its own weight. It is made from high-quality bauxite clinker, mullite and fused corundum, with pure calcium aluminate cement, corundum micro-powder and silicon micro-powder as binders. Cold crushing strength is minimum 60 to 85 MPa, refractoriness minimum 1790 °C and thermal shock resistance minimum 20 cycles at 900 °C water cooling.

Q11. When do you add steel fiber reinforcement to the lining?

Steel fiber reinforcement belongs where the damage is mechanical rather than pure abrasion. CH-NMJZ75, CH-NMJZ80 and CH-NMJZ85 give alumina minimum 75, 80 and 85 percent, with special-grade aluminum bauxite clinker or corundum aggregate and powder plus heat-resistant stainless steel fiber, binder and admixture. They reach modulus of rupture minimum 16 to 20 MPa and cold crushing strength minimum 70 to 100 MPa, with normal wear maximum 8 cm³ and thermal shock resistance minimum 20 cycles at 900 °C water cooling. Typical placements are CFB boiler furnace wall and furnace roof, cement kiln kiln mouth, cooling machine and feed tank.

Acid Resistant and Chemical Service Materials

Q12. How do I choose a grade of acid-resistant brick?

Three NSZ chemistry grades are available, and the choice is driven by bulk density. CH-NSZ1.0 with bulk density maximum 1.0 g/cm³ is for general acid regeneration process furnace lining service, CH-NSZ1.3 at maximum 1.3 g/cm³ is for higher-demand service, and CH-NSZ1.8 at maximum 1.8 g/cm³ is for the highest-demand service. Across all three grades the acid proof is minimum 96 percent, water absorption is maximum 12 to 15 percent, cold crushing strength is minimum 10 to 20 MPa, and heating line change is maximum 0.1 percent at 300 °C. Moving up the density scale buys mechanical strength, not acid resistance.

Q13. What do I use inside acid vessels, gasifiers and carbon black reactors?

Two very different materials cover chemical service, and the medium decides which. Acid-resistant castable is a chemical barrier against strong acid corrosion: it uses special water glass or other acid-resistant chemical binders and survives stably on the inner walls of harsh chemical equipment containing sulfuric acid (H₂SO₄), hydrochloric acid (HCl) and other acidic gases or liquids without being powdered or peeled off. Chrome corundum brick, mixing high-purity alumina with chromium oxide (Cr₂O₃), gives extremely high strength and an abnormally high corrosion resistance that can hardly be penetrated or dissolved in coal chemical water-coal slurry gasifiers, carbon black reactors and refining environments with severe acid and alkaline slag erosion.

Q14. Which mortar goes into the joints of a refractory brick lining?

Refractory mortar comes in seven grades, and you match the chemistry to the brick rather than to the acid. CH-GA88 with alumina minimum 88 percent is for high alumina brick masonry joints, CH-GACr88 with Cr₂O₃ plus Al₂O₃ minimum 88 percent is for corundum-chrome brick, CH-GM85 with MgO plus Al₂O₃ minimum 85 percent is for magnesia-alumina brick, and CH-GMCr85 is the chrome-enhanced version. CH-GT85, CH-GT80 and CH-GT70 carry alumina minimum 85, 80 and 70 percent. Across the family refractoriness is minimum 1500 to 1690 °C, hardening time is 60 to 180 seconds and adhesive strength is minimum 1 MPa, with erosion and wash-out resistance from high-temperature liquid deciding the campaign.

Q15. Should I use refractory clay or a high temperature binder as the bonding medium?

They do different jobs. Refractory clay, also called soft clay, is the plastic bonding medium for masonry jointing of clay and high alumina bricks: six grades CH-NN38, CH-NN42, CH-NN45, CH-LN55, CH-LN65 and CH-LN75 give alumina minimum 38 up to 75 percent with refractoriness minimum 1630 to 1790 °C and application temperature 1200 °C for NN grades, 1400 °C for LN grades. High temperature binder is the adhesive for industrial furnace masonry joints: grades GNJ42, GNJ32, GNJ46 and GNJ36 with alumina minimum 32 to 46 percent, modulus of rupture minimum 1 MPa after 1400 °C firing for 3 hours and maximum service temperature 1450 to 1600 °C.

Q16. Which refractory cement do you bond castables with?

Four grades cover the binder job. A600 with alumina minimum 50 percent serves general refractory castable binder service, A700 with alumina 50 to 60 percent is for higher demand, A900 with alumina minimum 53.5 percent is for high demand, and CA-70 with alumina 68.5 to 70.5 percent is for the highest demand, with CaO 28.5 to 30.5 percent. Silica is maximum 0.5 to 7.8 percent and iron oxide maximum 0.2 to 2.5 percent. Initial setting is 45 to 180 minutes with final setting maximum 150 to 360 minutes, and cold crushing strength reaches 40 to 72 MPa at 24 hours and 45 to 82 MPa at 72 hours.

Ceramic Fibre Products and Insulation

Q17. Which ceramic fiber form belongs in which zone of the furnace?

Six forms, six jobs. Ceramic Fiber Blanket is the furnace lining, roof, expansion joint, furnace door and high temperature pipe insulation, and it is the easiest to cut on site, at 95 to 160 kg/m³. Ceramic Fiber Board is the machined version for kiln and furnace walls and ceramic kiln fire blocking, at 200 to 600 kg/m³. Ceramic Fiber Bulk is loose fill for furnaces, equipment and pipelines. Ceramic Fiber Felt is the soft form for expansion joint fillers and high temperature gaskets. Ceramic Fiber Module is the compressed block at 150 to 250 kg/m³. Ceramic Fiber Shaped Pieces are vacuum molded burner blocks and observation holes.

Q18. Ceramic fiber blanket or ceramic fiber board — how do I choose?

Use blanket where the material has to be cut and fitted on site and where volume density must stay low. All five blanket grades, CH-XWT40, CH-XWT45, CH-XWT48, CH-XWT50 and CH-XWTZ15, run a volume density of 95 to 160 kg/m³, thermal conductivity maximum 0.14 to 0.28 W/m·K and heating shrinkage maximum 3 percent. Board is the denser, more precise form at 200 to 600 kg/m³ with the same conductivity ceiling, heating shrinkage maximum 1.5 percent after 900 to 1300 °C drying for 24 hours, and sizes of 600 mm by 400 mm by 10 to 50 mm or 900 mm by 600 mm by 10 to 50 mm.

Q19. Which ceramic fiber grade belongs in the highest-demand zone?

Each fiber family runs five grades, and the fifth is the one for the worst zone. Four are aluminum silicate based: CH-XWT40 at alumina 40 to 44 percent, CH-XWT45 at 44 to 46 percent, CH-XWT48 at 46 to 50 percent, and the high alumina grade CH-XWT50 at 50 to 60 percent. The fifth is zirconia containing, at alumina 30 to 35 percent with zirconia minimum 15 percent, sold as CH-XWTZ15 for blanket, CH-XWKZ15 for board and module, CH-XWMZ15 for bulk, CH-XWZZ15 for felt and CH-XWJZ15 for shaped pieces. Service temperature is maximum 1000 to 1350 °C, iron oxide maximum 0.5 to 1.2 percent and alkali maximum 0.2 to 0.5 percent.

Q20. Ceramic fiber castable for a reformer or a hydrogen furnace?

Where you need a cast hot face rather than a blanket, ceramic fiber castable is the answer. Five grades: CH-XWC06, CH-XWC08, CH-XWC10, CH-XWC12 and CH-XWC15, with alumina minimum 20, 25, 30, 35 and 35 percent and alumina plus silica minimum 80 percent for all five. Service temperature is 600 to 1100 °C depending on grade, cold crushing strength minimum 1.0 to 6.0 MPa after 110 °C drying for 24 hours, thermal conductivity maximum 0.16 to 0.28 W/m·K, permanent linear change maximum 1.0 percent after 600 °C firing for 3 hours and cure time maximum 10 hours. It serves reforming furnaces, hydrogen furnaces, firing blocks, burning blocks and burner blocks.

Q21. Which insulating brick goes behind the working layer?

Four families cover the back-up layer, and the choice follows the temperature. Clay insulating brick in grades NG-0.5 to NG-1.0 has bulk density minimum 0.5 to 1.0 g/cm³, cold crushing strength minimum 1.5 to 3.4 MPa, thermal conductivity maximum 0.18 to 0.50 W/m·K at 350 °C and maximum service temperature 1150 to 1300 °C. High alumina insulation brick in grades CH-LG0.6, CH-LG0.8 and CH-LG1.0, all at alumina minimum 48 percent, raises that to 1300 to 1380 °C. Mullite insulation brick in JM23, JM26 and JM28 grades reaches alumina minimum 67 percent, and light weight silica brick CH-QZ1.2 keeps refractoriness minimum 1670 °C at silica minimum 91 percent.

Wear Resistant Castables and Plastics

Q22. Which light weight castable or gunning mix goes behind the working layer?

Light weight castable is the cast back-up layer: seven QJ grades from CH-QJ0.5 at bulk density 0.5±0.1 g/cm³ up to CH-QJ1.8 at 1.8±0.1 g/cm³, with cold crushing strength minimum 1.5 to 8 MPa after 110 °C drying for 24 hours, cold crushing strength after burning minimum 1.5 to 7 MPa at 500 to 1200 °C, thermal conductivity maximum 0.19 to 0.80 W/m·K at the 800 °C hot side and maximum service temperature 700 to 1350 °C. Light weight gunning mix, grades CH-QP0.7, CH-QP1.0 and CH-QP1.4 at 0.75±0.1 to 1.5±0.1 g/cm³, does the same job where formwork cannot reach, with good adhesion and low rebound.

Q23. What insulation do I use when the back-up has to carry a higher temperature?

Alumina hollow sphere products are the answer when the back-up layer must still carry real temperature. They are made from alumina hollow spheres, corundum powder and calcined powder, homogenized, shaped and sintered at high temperature, keeping a low thermal conductivity and a small bulk density. Three KXQ grades: CH-KXQ88 at alumina minimum 88 percent, CH-KXQ98 at minimum 99 percent, and the CH-KXQ98 Sialon grade at zirconia minimum 9.8 percent. Bulk density is 1.30 to 3.0 g/cm³, cold crushing strength minimum 8 to 15 MPa, load softening temperature minimum 1650 to 1700 °C at 0.2 MPa and maximum service temperature 1650 to 2200 °C.

Q24. What goes into the furnace bottom of a high-wear unit?

Slag and abrasion resistant castable for furnace bottom and other high wear resistance parts is produced from corundum and mullite with compound ultra-fine powders added. Three grades: CH-BLN70, CH-BLN75 and CH-BLN80, carrying alumina minimum 70, 75 and 80 percent. Bulk density is minimum 2.25 to 2.75 g/cm³ after 110 °C drying for 24 hours, cold crushing strength minimum 40 to 75 MPa, permanent linear change maximum 0.5 percent after 1400 °C firing for 3 hours, and water requirement 5 to 7 percent. Maximum service temperature is 1400 to 1500 °C, and the bottom zone is where wear decides the campaign life.

Q25. Which brick belongs in a transition zone rather than a working layer?

Two aluminosilicate families cover zones where a working layer is not needed. Silicon mullite brick is made from bauxite clinker and silicon carbide, for the cement kiln transition zone, cooling zone and kiln mouth: CH-GMZ65 at alumina maximum 65 percent, CH-GMZ63 at maximum 63 percent and CH-GMZ60 at maximum 60 percent, all with refractoriness minimum 1790 °C, bulk density minimum 2.50 to 2.60 g/cm³ and refractoriness under load at 0.2 MPa minimum 1550 to 1680 °C. Sillimanite brick CHGX-60, at alumina 60 to 65 percent, serves kiln lining and insulation layer duty with apparent porosity maximum 18 percent and thermal shock resistance minimum 30 cycles at 1100 °C water cooling.

Q26. We make our own castables and brick. Which raw material grades should we specify?

Two raw materials decide most of the end product. Refractory grade bauxite in five grades RK70, RK75, RK80, RK85 and RK87 gives alumina minimum 70 to 87 percent with iron oxide maximum 1.5 to 2 percent, bulk density 2.95 to 3.35 g/cm³ and water absorption maximum 3 to 5 percent, and it feeds high alumina brick, high alumina castable, mullite brick and andalusite brick production. Alumina powder comes as NX-1, NX-2, NX-3 and HX-1 with alumina minimum 99.0 to 99.7 percent, true specific gravity minimum 3.93 to 3.95 g/cm³ and primary crystal size 1 to 4 micrometer, in sizes from 80 mesh to 5000 mesh.

Q27. How do you coat the flue and the pipe runs of a power unit?

The flue and pipe runs fail differently from the furnace, because they see gas flow and particle carry-over rather than process charge. Refractory spray coating material, an aluminum-silicon series product, is used for the high temperature pipelines and flue systems of kilns such as blast furnaces and hot blast stoves. Two grades are offered, CH-PTL40 with alumina minimum 40 percent and CH-PTL45 with alumina minimum 45 percent, in light, medium or heavy grade. Bulk density after 1300 °C burning is minimum 1.0 to 1.95 g/cm³, refractoriness minimum 1530 to 1610 °C and permanent linear change plus or minus 1.0 percent after 1300 to 1400 °C firing for 3 hours.

Power and Petrochemical Project Service

Q28. What data do you need from me before you recommend a material?

Six pieces of operating data. Equipment type and the specific location inside it. Extreme and normal operating temperatures. Furnace atmosphere, oxidizing or strongly reducing. Chemical composition of the slag and flux, including acidity or alkalinity. Thermal cycling heating and cooling frequency. And your target campaign life. With those, our engineering team recommends the matching material formula, the masonry thickness and the installation method, through 3D CFD fluid simulation or Solidworks 3D. Sending the furnace drawing, lining design, furnace capacity and operating temperature data with your enquiry shortens that loop considerably.

Q29. Do you supply the lining design and brick layout, or only the bricks?

You get the design, not only the bricks. A 3D refractory lining design and simulation package covers custom special-shaped brick and precast block engineering drawings, thermal stress and mechanical load analysis of complex parts, precise installation brick layout drawings, a bill of materials accurate to each brick, and on-site masonry supervision by senior engineers. Behind that sits 3D CFD fluid simulation: before bricks go into production, combustion chamber airflow, combustion air and high-temperature flue gas trajectories are simulated over one to two weeks, which eliminates combustion dead corners, optimizes heat distribution uniformity and protects the refractory from biased flow erosion.

Q30. Can you show me a completed power project with references?

Two reference projects in hot blast stove work. The first is a benchmark turnkey refractory package for Jiuquan Steel Group's 1,080 m³ large hot blast stove, where 3D CFD fluid simulation optimized air and flue gas trajectories and four product categories were customized by zone: high alumina bricks at 70 percent alumina and above, silica bricks at 95 percent and above, and low creep andalusite. It followed the six-step one-stop service of design, manufacturing, installation, commissioning, after-sales and hot repair, with a service life guarantee of more than 15 years. The second, for Fujian Dingxin Steel, added one to two weeks of 3D simulation before production and hot commissioning training.

Q31. What goes into the regenerator of a hot blast stove, and how do the grades differ?

Refractory balls, made from industrial alumina and refractory kaolin, formed and calcined at high temperature, are the checker material in a hot blast stove regenerator. Ten grades are available and they split into three families: alumina-rich grades for the highest temperature duty, a magnesium-aluminum series with magnesium content from 8.5 to 55 percent, and a magnesium chromite series with magnesium content up to 85 percent, plus handmade high-strength aluminum and low creep grades. Maximum service temperature reaches 1900 °C for the alumina-rich grades, apparent porosity is 18 to 23 percent, bulk density 2.2 to 2.85 g/cm³ and refractoriness is 1790 °C across all ten grades.

Q32. Is the market moving from shaped brick to monolithic, and should I change my specification?

Material choice is moving in one direction. Monolithic materials, meaning bulk materials, castables and gunning mixes, are expected to exceed 45 percent of global consumption by 2030, and over 50 percent in developed countries, because they remove expensive brick firing cost, give on-site pumping and casting speed, remove the weak point a brick joint always is, and deliver batch consistency through microcomputer batching. Traditional clay-based and ordinary high-alumina refractories historically held 54 percent by volume, and non-clay high-end grades are growing fast. Expect your next power package specification to be reviewed toward monolithic.

Q33. How is the refractory qualified and cleared for a power project site?

Qualification is planned, not improvised. Third-party witnessed testing is open: we work with SGS, BV, CCIC and German TUV, whose experts can witness sampling, sample preparation and destructive pressing in our factory laboratory if you book five to seven days ahead. The export pack covers customs clearance at any port: stamped commercial invoice, detailed packing list, Certificate of Origin, physical and chemical quality certificate, MSDS, marine insurance certificate, original bill of lading or air waybill, and fumigation and phytosanitary certificates for wooden packaging.

Q34. What are you committed to after the power unit is commissioned?

The commitment is written, not implied: over 15 years of campaign life on hot blast stove core linings and 8 years in nonferrous smelting environments, plus 7×24 remote expert diagnosis and 3 to 5 days on site training your team on baking, hot repair technique and safety limits. We also inspect and evaluate the lining during each planned overhaul. Cold face temperature, the surface temperature of the outermost metal shell, is the daily indicator of insulation effectiveness; our targets are a ladle shell below 350 °C and a cement kiln shell below 350 °C. Wear rate is confirmed by residual thickness measurement at shutdown and chemical penetration analysis.

Industry Knowledge for Refractory Buyers

How is an ethylene cracking furnace lining structured?

The requirements are insulation, energy saving and thermal sensitivity together, so a composite multi-layer structure is used. The outermost layer is covered with ceramic fibre blanket. The middle layer is insulating fire clay brick or a light-weight insulating castable. The innermost hot face working layer, which takes the combustion gas flow erosion, is usually high-grade high alumina plastic or a high-strength light-weight castable.

What service life should I expect from ethylene cracking furnace linings?

It depends on the operating environment and the maintenance level. The ultra-lightweight ceramic fibre modules in the inner working area typically last 3 to 6 years, while traditional brick or castable heavy-duty insulating linings can last 5 to 10 years. Regular surface thermal anti-corrosion spraying can extend either figure further, so the maintenance plan matters as much as the material.

How do CFB boiler linings resist particle erosion?

A circulating fluidised boiler liner is built to survive dense coal and desulphurisation agent particles cycling at very high speed. It uses extremely high-density wear-resistant castables, wear-resistant plastics, and gunning mixes dedicated to hot-state emergency repair. The combination comprehensively protects the cyclone, target area and return feeder, which are the points where erosion concentrates.

How does acid-resistant castable protect chemical plant equipment?

It acts as a chemical barrier against strong acid corrosion. It uses special water glass or other acid-resistant chemical binders, and it survives on the inner walls of chemical equipment handling sulphuric acid, hydrochloric acid and other acidic gases or liquids without being powdered or peeled off by the acidic medium. Acid-resistant brick serves the same duty where a shaped unit is needed.

What are the key properties to compare in ceramic fibre products?

Volume density, thermal conductivity, service temperature and shrinkage are the four that decide the application. Low thermal conductivity is what makes the product worth using, and it is quoted at a stated reference temperature so the comparison is valid. The family spans ordinary grade at about 1,050 °C, zirconia-containing grade at 1,430 °C and polycrystalline alumina high-end fibre at 1,600 °C, with volume density in the 64 to 192 kg/m3 range for blanket and bulk forms.

What does a self-flowing castable buy you over a conventional castable?

It removes the vibration step. Self-flowing grades reach full density and full strength by gravity alone, so they suit complex geometry, confined spaces, thin sections and overhead work where a vibrator cannot be used or where access is limited. They also cut installation labour and cycle time, which matters on a shutdown schedule where every hour has a cost.

How should I specify refractory for a CFB boiler furnace wall and roof?

The furnace wall and roof take high-strength wear-resistant grades with high compressive and flexural strength, good volume stability and steel fibre reinforcement where thermal cycling is severe. The refractory surface of the CFB boiler is also continuously exposed to fast particle impact, so the material must be specified on wear resistance rather than on compressive strength alone. Normal wear volume is one of the parameters to check against the supplier's data.

Industrial Furnace Refractory

Questions: 37

Questions in this section
  1. Furnace Roof and Suspended Lining (4)
  2. Burner Block and Frame Brick (4)
  3. Load-Bearing Brick and Long-Life Furnace Parts (8)
  4. Plastic, Gunned and Cast Furnace Materials (5)
  5. Insulation and Light Weight Products (5)
  6. Industrial Furnace Project Service and Engineering (4)
  7. Industry Knowledge for Refractory Buyers (7)

Furnace Roof and Suspended Lining

Q1. My industrial furnace roof hangs over the burner zone. Do I use anchor brick or the same castable as the lining?

Anchor brick is made from the same base material as the lining castable, which is why it holds up in a suspended roof: good thermal shock resistance and high strength, with no chemistry mismatch against the castable behind it. Two grades are supplied, CH-MG48 with Al2O3 minimum 48 percent for general roof and suspended lining service and CH-MG55 with Al2O3 minimum 55 percent for higher-demand duty. Refractoriness is minimum 1730 to 1750 °C depending on grade, bulk density minimum 2.30 to 2.35 g/cm3, apparent porosity maximum 21 to 22 percent and cold crushing strength minimum 45 to 50 MPa. Send the roof drawing, furnace capacity and operating temperature and the grade is matched to them.

Q2. Do the charge gate, discharge gate and partition of an annular heating furnace need a different brick from the rest of the roof?

Yes, those zones are built with hanger brick, because the job there is to stop cold gas entering the working zone. The partition suspending bricks are produced with light weight mullite aggregate by low cement castables. Two grades are supplied, CH-DG1.8 and CH-DG2.0. Bulk density is minimum 2.45 to 2.6 g/cm3 and cold crushing strength minimum 15 to 25 MPa after 110 °C for 24 hours and 1200 °C for 3 hours. Permanent linear change is -0.8 to 0 percent for CH-DG1.8 and -0.6 to 0 percent for CH-DG2.0 after 1200 °C firing for 3 hours, so the gate lining shrinks slightly instead of growing into the frame, and the strength is lower than anchor brick, so specify it for gate duty rather than reusing a roof spec.

Q3. How much room do I leave for expansion in the roof lining, and what goes in the joint?

Leave the movement to the filler and fill it with something that can be crushed. Ceramic fibre paper, or a high-grade polycrystalline microporous board, goes into the reserved gaps in brick masonry. As the furnace heats up the bricks expand violently and squeeze each other, and the soft filler absorbs that destructive volume expansion so the rigid brick is not crushed and spalled by thermal compressive stress. Size the filler so it fills the gap and the lining can compress it as it expands. For reference, anchor brick and frame brick both limit permanent linear change to maximum 0.5 percent after 1400 °C firing for 3 hours, while plastic refractory for furnace lining allows maximum 0.6 percent after 1400 °C for 3 hours.

Q4. Which jointing material goes with which brick in the roof and wall masonry?

Match the jointing product to the brick and to the joint you are designing. Refractory clay is the plastic masonry clay for clay brick and high alumina brick masonry: six NN and LN grades from CH-NN38 at Al2O3 minimum 38 percent and refractoriness minimum 1630 °C to CH-LN75 at 75 percent and 1790 °C, with application temperature 1200 °C on NN grades and 1400 °C on LN grades. Refractory mortar, for ladle brick joints, has seven grades including CH-GA88 and CH-GACr88 at Cr2O3 plus Al2O3 minimum 88 percent, refractoriness minimum 1500 to 1690 °C and hardening time 60 to 180 seconds. High alumina refractory mortar runs CH-LN55 to CH-LN75 at refractoriness minimum 1770 to 1790 °C, and high temperature binder comes as four GNJ grades, Al2O3 minimum 32 to 46 percent, maximum service temperature 1450 to 1600 °C, packed in 25 or 30 kg bags.

Burner Block and Frame Brick

Q5. Burner block and frame brick sit in the same furnace. Where do I change material, and which grade do I use?

Burner block is the hot-face piece at the burner: corundum-mullite based and mullite based, in two grades, CH-SZ65 with Al2O3 minimum 65 percent for general burner lining service and CH-SZ75 with Al2O3 minimum 75 percent for higher-demand service. Bulk density is minimum 2.45 to 2.6 g/cm3, cold crushing strength minimum 40 to 65 MPa at 110 °C for 24 hours and 1500 °C for 3 hours, and permanent linear change maximum 0.5 percent after 1500 °C for 3 hours. Frame brick is the structural connector between the lining frame and the burner block: three BK grades, CH-BK55 at Al2O3 minimum 55 percent, CH-BK60 at 60 percent and CH-BK65 at 65 percent, with bulk density minimum 2.45 to 2.55 g/cm3, cold crushing strength minimum 35 to 60 MPa, permanent linear change maximum 0.5 percent after 1400 °C for 3 hours, and good abrasion and thermal shock resistance.

Q6. Can I get a shaped ceramic fibre burner block or observation-hole plug made to my drawing?

Yes. Ceramic fibre shaped pieces are the answer wherever the insulation has to hold a specific geometry: observation holes, temperature measuring holes, pressure measuring holes, burner blocks, furnace doors, electric heating wire supporters, hot pipe lining, and molten aluminium collectors and grooves. They are made from refractory fibre by vacuum molding, and special moulds are designed for the part. Five grades are offered, from CH-XWJ40 at Al2O3 40 to 44 percent through CH-XWJ50 high alumina at 50 to 60 percent and CH-XWJZ15 with ZrO2 minimum 15 percent. Volume density is 200 to 600 kg/m3, cold crushing strength minimum 0.2 MPa, heating shrinkage maximum 2 percent after 900 to 1300 °C for 24 hours and service temperature maximum 1000 to 1350 °C.

Q7. For the arc furnace cap and the ladle furnace triangle area, do I cast in place or lift in a factory-made part?

Both exist and the decision is mostly about the shutdown. The special castable for arc furnace cap comes as DLD75 to DLD92, Al2O3 minimum 75 to 92 percent, with bulk density minimum 2.6 to 3.1 g/cm3 after 110 °C for 24 hours, flexural strength minimum 8 to 13 MPa, compressive strength minimum 60 to 100 MPa and maximum service temperature 1450 to 1700 °C. For the LF refining furnace electrode delta area, a factory-customized precast part in ultra-high refractoriness corundum-spinel or corundum-mullite installs extremely quickly and gives thermal shock and spalling resistance far superior to on-site casting under high-temperature arc radiation. The EAF tilting steel pouring spout takes a large factory-precast corundum-spinel block for accurate spout dimensions and concentrated steel flow without dispersion.

Q8. How do I line the flue and the hot pipework leaving the burner zone?

The refractory spray coating material is an aluminium-silicon series product for high temperature pipelines and flue systems in kiln furnaces such as blast furnaces and hot blast stoves, and it comes in light, medium or heavy grade according to the service. Two chemistry grades are supplied, CH-PTL40 at Al2O3 minimum 40 percent and CH-PTL45 at minimum 45 percent. Refractoriness is minimum 1530 to 1610 °C, bulk density minimum 1.0 to 1.95 g/cm3 after 1300 °C burning, modulus of rupture minimum 4.0 to 4.4 MPa after 110 °C drying and minimum 0.5 MPa after 1300 to 1400 °C hot forming, and permanent linear change ±1.0 percent after 1300 to 1400 °C firing for 3 hours. Adhesion is certain and the rebound rate is low, so material is not lost as overspray.

Load-Bearing Brick and Long-Life Furnace Parts

Q9. Which brick belongs in the burning zone of a cement rotary kiln, and what life should I budget?

The burning zone is the core area with the highest temperature, the heaviest thermal load and the strongest liquid clinker corrosion in the whole kiln. It mainly uses direct-bonded magnesia-chrome brick, high-quality magnesia-alumina spinel brick, or dolomite brick, and these materials adhere to the kiln coating and protect themselves. Magnesia-chrome brick life is usually 6 to 12 months, while high-quality dolomite or spinel brick can reach 8 to 18 months. Elsewhere in the furnace, high grade magnesia brick runs MZ-90 to MZ-97 by MgO content from minimum 90 percent to minimum 97 percent, with bulk density minimum 2.9 to 3.0 g/cm3, apparent porosity maximum 18 to 20 percent, cold crushing strength minimum 40 to 50 MPa and refractoriness under load minimum 1500 to 1650 °C at 0.2 MPa loading.

Q10. How do I read refractoriness under load, and why does it matter more than refractoriness?

Refractoriness under load is the number that tells you whether the material can carry the weight of the structure above it at temperature, and it is measured differently from plain refractoriness. Under a specified constant pressure load, standard usually 0.2 MPa, the sample is heated continuously at 2 to 5 °C per minute until it begins to deform and collapse, which is recorded as 0.5 to 1 percent compression deformation. The published figures to compare are: high grade magnesia brick minimum 1500 to 1650 °C at 0.2 MPa, silicon mullite brick minimum 1550 to 1680 °C at 0.2 MPa, high alumina brick load softening temperature minimum 1420 to 1520 °C and fire clay brick minimum 1300 to 1400 °C at 0.2 MPa. Compare like with like on the data sheet.

Q11. Is my furnace wall better in fire clay brick, high alumina brick or common silica brick?

Start from what touches the lining. Fire clay brick is a weakly acidic refractory, mainly kaolinite with 6 to 7 percent impurities of potassium, sodium, calcium, titanium and iron oxides, and firing converts the kaolinite to mullite crystallization; it resists acidic slag and acid gases and is less resistant to alkaline substances. Across eight N grades refractoriness is minimum 1580 to 1750 °C, load softening temperature minimum 1300 to 1400 °C at 0.2 MPa, apparent porosity maximum 22 to 28 percent and cold crushing strength minimum 15 to 30 MPa. High alumina brick is the harder alkaline-resistant option at Al2O3 minimum 48 to 75 percent with refractoriness minimum 1750 to 1790 °C and cold crushing strength minimum 40 to 54 MPa, while common silica brick CH-GZ95 and CH-GZ94 hold refractoriness 1710 °C at cold crushing strength 29.4 MPa and 24.5 MPa.

Q12. What goes in the transition zone, cooling zone and kiln mouth of a cement kiln?

Silicon mullite brick is made from high-grade bauxite clinker and high-quality silicon carbide fired at high temperature. Three grades are offered, CH-GMZ65, CH-GMZ63 and CH-GMZ60, all with Al2O3 maximum 65, 63 and 60 percent and refractoriness minimum 1790 °C. Bulk density is minimum 2.50 to 2.60 g/cm3, apparent porosity maximum 20 to 21 percent, cold crushing strength minimum 80 to 95 MPa, high temperature modulus of rupture minimum 8 to 15 MPa at 1450 °C, refractoriness under load minimum 1550 to 1680 °C at 0.2 MPa and thermal shock resistance minimum 10 to 15 cycles at 1100 °C. Where the lining is a kiln lining and insulation layer that is not eroded by molten liquid, sillimanite brick CHGX-60 at Al2O3 60 to 65 percent and SiO2 30 to 35 percent gives load softening minimum 1550 °C at 0.2 MPa and thermal shock minimum 30 cycles at 1100 °C water cooling.

Q13. How is a tundish lined, and why does the working lining differ from the permanent layer?

The tundish is the core hub of the continuous casting system, and each layer does a different job. The permanent layer uses alumina-magnesia castable. The working lining currently mainly uses magnesia-based or neutral dry vibrating material, with no water added, giving rapid baking and demolding. The surface is covered with acidic or alkaline tundish covering agent for insulation and inclusion absorption, and internal flow control uses dams, weirs and various flow stabilizer precast parts. The chemistry choice follows the same pattern as the general magnesia brick grades, where MZ-95 at MgO minimum 95 percent with SiO2 maximum 2.50 percent and CaO maximum 2.0 percent, and MZ-97 at MgO minimum 97 percent with SiO2 maximum 1.20 percent and CaO maximum 1.50 percent, are the high and highest-demand grades.

Q14. Do I need a special brick for an acid regeneration process furnace?

Yes, in power and petrochemical service the lining is judged on acid resistance rather than temperature alone. Three NSZ grades are supplied, CH-NSZ1.0, CH-NSZ1.3 and CH-NSZ1.8, defined by bulk density maximum 1.0, 1.3 and 1.8 g/cm3. All three give acid proof minimum 96 percent, water absorption maximum 12 to 15 percent depending on grade, cold crushing strength minimum 10 to 20 MPa at normal temperature and heating line change maximum 0.1 percent at 300 °C. The family delivers acid resistance, high temperature resistance, high strength and anti-scour performance for the acid regeneration process furnace lining, which is what keeps the unit running between shutdowns.

Q15. I press my own brick. Which bauxite and alumina powder should I specify?

The raw material spec is where the grade is won. Refractory grade bauxite comes as RK70 to RK87, Al2O3 minimum 70 to 87 percent, with Fe2O3 maximum 1.5 to 2 percent, TiO2 maximum 4 percent on RK80, RK85 and RK87, CaO plus MgO maximum 0.4 to 0.6 percent, K2O plus Na2O maximum 0.4 to 0.6 percent, bulk density 2.95 to 3.35 g/cm3 and water absorption maximum 3 to 5 percent, supplied as 0 to 0.3 mm up to 5 to 8 mm aggregate and 100, 200 or 325 mesh powder. Alumina powder comes as NX-1, NX-2, NX-3 and HX-1 at Al2O3 minimum 99.7 down to 99.0 percent, with Na2O up to 0.10 to 0.20 percent, true specific gravity minimum 3.93 to 3.95 g/cm3 and alpha-Al2O3 minimum 94 to 95 percent.

Q16. What do I put in the regenerator of a hot blast stove, and which ball grade fits?

Refractory balls for heat storage in hot blast stoves are made from industrial alumina and refractory kaolin, formed and calcined at high temperature, and ten grades are supplied. Maximum service temperature reaches 1900 °C for the alumina-rich grades, including the mechanism high-strength high-density aluminum ball at alumina content 75 percent or higher. The magnesium-aluminum series carries magnesium content from 8.5 to 55 percent, and the magnesium chromite series reaches magnesium content up to 85 percent, with the handmade high-strength aluminum ball and handmade low creep ball as further options. Apparent porosity ranges 18 to 23 percent and bulk density 2.2 to 2.85 g/cm3, with refractoriness 1790 °C across all ten grades. The same family serves shifting furnaces, reforming furnaces, hydroconverters, desulfurization tanks and methanol furnaces in fertilizer plants.

Plastic, Gunned and Cast Furnace Materials

Q17. How do I choose plastic refractory for the furnace roof, wall and fume pipe?

One grade covers this service: CH-blS50 with Al2O3 minimum 50 percent, produced from bauxite and mullite with suitable binders and additives. It is engineered for industrial furnace roof, wall and fume pipe lining, and the reason it fits is the combination of good installation property, good thermal shock resistance, low thermal expansion and good thermal insulation. Bulk density is minimum 2.25 g/cm3 after 110 °C drying for 24 hours, cold crushing strength minimum 16 MPa after 110 °C for 24 hours and minimum 30 MPa after 1400 °C firing for 3 hours, and permanent linear change maximum 0.6 percent after 1400 °C for 3 hours. On site it is installed by pneumatic ramming with air picks, so ask for the installation procedure with the order.

Q18. Should my roof lining be gunned or shotcreted, and what grade do I use?

The two methods are not interchangeable. Gunning mostly uses semi-dry material, driven by high-pressure air at high speed onto the red-hot old furnace lining surface, where it sinters instantly; it is used for thin layer coverage and emergency hot repair. Shotcreting pumps a wet slurry of high density with accelerators, has extremely low rebound, and can spray extremely thick permanent structural layers in one pass, which suits new large furnace chambers or an overall cold overhaul. Both construction speeds far exceed traditional formwork casting. Where a product has to serve insulation lining and working lining at once, light weight gunning mix comes as CH-QP0.7, CH-QP1.0 and CH-QP1.4 at bulk density 0.75, 1.1 and 1.5 g/cm3 with ±0.1 tolerance, cold crushing strength minimum 2 to 6 MPa and thermal conductivity maximum 0.30 to 0.54 W/m·K at 800 °C hot side.

Q19. Can you hot-repair a running furnace, and how long does a shutdown really take?

Hot repair is a planned part of the service rather than an exception. High-temperature fast-setting castables are used for emergency repair of sudden furnace penetration, and high-pressure gunning mix solutions restore slag line thickness within planned schedules. Standard spare parts are held in stock for shipment within 48 hours. During ladle operation, spray hot repair is implemented every 5 to 10 heats using gaps, which has been proven to stably extend overall ladle campaign life by more than 30 percent. On the bigger shutdowns, local rapid hot repair of the slag line or impact pad takes only 6 to 10 hours, and with a fully modular precast block lifting solution the cold repair replacement time drops from several days to within 6 to 12 hours.

Q20. What goes into the furnace bottom and the kiln coal injection pipe, and how much water does the castable take?

Two wear zones, two castable families. For the furnace bottom and other high wear resistance parts, the slag and abrasion resistant castable is offered as CH-BLN70, CH-BLN75 and CH-BLN80 at Al2O3 minimum 70, 75 and 80 percent, with bulk density minimum 2.25 to 2.75 g/cm3 after 110 °C for 24 hours, cold crushing strength minimum 40 to 75 MPa, permanent linear change maximum 0.5 percent after 1400 °C for 3 hours, water requirement 5 to 7 percent and maximum service temperature 1400 to 1500 °C. The cement kiln coal injection pipe uses CH-PJZ68, CH-PJZ72 and CH-PJZ78 at Al2O3 minimum 68, 72 and 78 percent, bulk density minimum 2.6 to 2.8 g/cm3, modulus of rupture minimum 8 to 12 MPa, cold crushing strength minimum 60 to 90 MPa and permanent linear change ±0.5 percent after 1400 °C for 3 hours.

Q21. Is the industry moving away from shaped brick toward monolithic materials, and should I change my specification?

Yes, the proportion of monolithic materials, meaning bulk materials, castables and gunning mixes, is surging and is expected to exceed 45 percent of global consumption by 2030, even over 50 percent in developed countries. The core driving logic is that monolithic eliminates the expensive and time-consuming brick high-temperature firing cost, that on-site pumping and casting construction speed creates a dimensional advantage, that a joint-free lining has no fatal weak point of brick joints, and that microcomputer batching brings extreme batch consistency. That is a reason to price a monolithic option against your brick specification at the next quotation, not a reason to change a running furnace on its own.

Insulation and Light Weight Products

Q22. Which insulating brick belongs behind the working layer, and what are the limits of each family?

Three families sit behind the hot face, and the choice follows the temperature of the zone. Mullite insulation brick covers eight JM23, JM26 and JM28 grades at Al2O3 minimum 48 to 67 percent, bulk density minimum 0.6 to 1.2 g/cm3, cold crushing strength minimum 1.5 to 5.0 MPa, thermal conductivity maximum 0.2 to 0.4 W/m·K at average 350 °C and thermal shock resistance minimum 10 to 20 cycles at 1100 °C water cooling. Clay insulating brick is the four NG grades at bulk density minimum 0.5 to 1.0 g/cm3, load softening minimum 1160 to 1300 °C at 0.1 MPa, maximum service temperature 1150 to 1300 °C and Fe2O3 maximum 2.0 to 2.5 percent. Light weight silica brick CH-QZ1.2 at SiO2 minimum 91 percent keeps refractoriness minimum 1670 °C with load softening start minimum 1520 °C at 0.1 MPa, at bulk density 1.2 g/cm3.

Q23. Ceramic fibre blanket, module or shaped piece: which format do I order?

The chemistry ladder is the same in all three formats, so the format follows the geometry of the job. Blanket, module and shaped piece grades run from aluminium silicate at Al2O3 40 to 44 percent, through 44 to 46 and 46 to 50 percent, to the high alumina grade at 50 to 60 percent, plus the zirconia grade at Al2O3 30 to 35 percent with ZrO2 minimum 15 percent. Blanket is needled and easy to cut, volume density 95 to 160 kg/m3, thermal conductivity maximum 0.14 to 0.28 W/m·K, heating shrinkage maximum 3 percent, supplied 7200 by 600 mm in 12, 20, 25, 40 or 50 mm thicknesses. Modules are compressed blocks at 150 to 250 kg/m3 with heating shrinkage maximum 1.5 percent after 900 to 1300 °C for 24 hours, for firing and burning blocks. Shaped pieces are vacuum molded at 200 to 600 kg/m3 with cold crushing strength minimum 0.2 MPa and heating shrinkage maximum 2 percent, and the size is made to your drawing.

Q24. Bubble alumina or bubble alumina brick: which do I use behind the hot face?

Bubble alumina is the hollow sphere aggregate for lightweight insulating castable, lightweight insulating brick and high temperature furnace back-up lining, and also for petrochemical reformer insulation. Two grades are supplied: the high purity grade at Al2O3 minimum 99 percent with SiO2 maximum 0.2 percent, Fe2O3 maximum 0.1 percent and Na2O maximum 0.3 percent, and the high strength grade at Al2O3 minimum 98.5 percent with SiO2 maximum 1 percent, Fe2O3 maximum 0.08 percent and Na2O maximum 0.25 percent. Stacking density is 0.4 to 1 g/cm3, size 0 to 7 mm, rate of reduction maximum 15 percent and maximum working temperature 1825 °C. As a finished brick, bubble alumina brick comes as CHSAH99, CHAH99, CHAH90 and CHAH85 at Al2O3 minimum 99.3 down to 85 percent, bulk density 1.4 to 1.9 g/cm3, cold crushing strength minimum 12 to 18 MPa, initial softening temperature under load minimum 1700 °C and thermal conductivity 0.55 to 0.75 W/(m·K).

Q25. What is the difference between alumina hollow sphere products and the other hollow sphere products?

Alumina hollow sphere products are sintered shapes rather than loose aggregate: alumina hollow spheres, corundum powder and calcined powder are homogenized, shaped and sintered at high temperature. Three grades are supplied, CH-KXQ88 at Al2O3 minimum 88 percent for high-temperature kiln working lining, CH-KXQ98 at minimum 99 percent for higher-demand working lining, and the CH-KXQ98 Sialon grade with ZrO2 minimum 9.8 percent for the highest-demand service. SiO2 is maximum 0.2 percent and Fe2O3 maximum 0.15 to 0.3 percent. Bulk density is 1.30 to 3.0 g/cm3, cold crushing strength minimum 8 to 15 MPa, load softening temperature minimum 1650 to 1700 °C at 0.2 MPa, reheating line change maximum ±0.2 to 0.3 percent after 1600 °C for 3 hours, thermal expansion coefficient approximately 8.0 to 8.6 times 10 to the minus 6 per °C at 1300 °C, thermal conductivity maximum 0.5 to 1.0 W/m·K at 800 °C and maximum service temperature 1650 to 2200 °C.

Q26. Which light weight castable grade do I use for the insulation layer, and how do I know the insulation is working?

Seven QJ grades are keyed by bulk density, from CH-QJ0.5 at 0.5±0.1 g/cm3 for the lowest temperature service up to CH-QJ1.8 at 1.8±0.1 g/cm3, and the grade must be matched to the zone temperature. Bulk density is 0.5±0.1 to 1.8±0.1 g/cm3 after 110 °C drying for 24 hours, cold crushing strength minimum 1.5 to 8 MPa after 110 °C for 24 hours and minimum 1.5 to 7 MPa after burning at 500 to 1200 °C, thermal conductivity maximum 0.19 to 0.80 W/m·K at 800 °C hot side and maximum service temperature 700 to 1350 °C. The result is checked from the cold face: the surface temperature of the outer shell of the lining, where the targets are ladle shell below 350 °C, cement kiln shell below 350 °C and ultra-high-power electric arc furnace shell below 250 °C.

Industrial Furnace Project Service and Engineering

Q27. How is each material actually installed on my furnace?

The installation method is matched to the material system. Shaped bricks are laid in a staggered masonry with special fireclay mortar, with precise expansion joints reserved and steel strips or anchors for fastening. Castables are force mixed, vibrated at high frequency after mold filling, wet cured and baked on a controlled curve. Plastics are pneumatically rammed with air picks. Gunning mixes are sprayed at high pressure. Precast blocks are factory customized and lifted and welded directly on site. Senior masons set quality control points throughout the process for dimensional and specification verification, so the check on brick dimensions and joint gaps is part of the installation rather than a separate inspection afterwards.

Q28. How do I mix, cure and dry a new castable lining without cracking it?

Mixing discipline comes first. Manual turning and free-fall drum concrete mixers are strictly prohibited; a strong paddle-type or planetary forced mixer must be used. Add the metered quantity of pure water according to the product data sheet, where low-cement castables typically take only 4.5 to 7.5 percent, and mix quickly for 3 to 5 minutes until the slurry is uniform. Once the slurry begins to set, no secondary water addition and remixing is allowed, or the strength will plummet. After installation and demolding, cover with wet sacks or spray curing agent for at least 24 hours of natural curing. Drying and baking follow the curve: 20 to 30 °C per hour to 200 °C with long holding to exhaust moisture, then 30 to 50 °C per hour to the operating temperature, so a 200 mm thick heavy-duty castable needs a full preheating curve of 24 to 36 hours.

Q29. How long can I store castable, plastic and precast blocks on site?

Storage is governed by the binder, so the rule follows the product type. Dry bagged moisture-proof castables are stored indoors in a dry, ventilated place for 6 to 12 months. Plastics containing liquid binders have a shorter shelf life, usually 3 to 6 months. Precast blocks that have been thoroughly high-temperature baked and shaped have almost no shelf life limit, provided they are kept dry. Order on that basis rather than on a general site storage rule, because a plastic batch that has passed its shelf life loses the installation property that makes it work in the first place.

Q30. What quality control do I get before the material ships and after the furnace is running?

Both ends of the project are covered. For complex special-shaped assemblies such as blast furnace tuyere combined bricks, the 100 percent factory pre-assembly process builds a platform in the workshop to the actual dimensions 1 to 1 and completely simulates the on-site assembly of the finished bricks; engineering drawing dimensions and reserved gaps are checked brick by brick, then the parts are spray coded and packed so there are truly zero fit problems at the construction site. After delivery and stable operation, the after-sales technical team provides professional on-site inspection and evaluation during your quarterly or semi-annual planned shutdown maintenance windows, and issues lining wear diagnosis and next-step hot maintenance guidance reports.

Industry Knowledge for Refractory Buyers

How do I select refractory for a suspended furnace roof?

A suspended roof is the most demanding position in an industrial furnace because it carries its own weight at high temperature. Anchor brick and frame brick are produced from the same base as the lining castables and are characterised by good thermal shock resistance and high strength. Selection must be made on refractoriness under load rather than on refractoriness, since a roof that softens will drop.

What is the role of the burner block?

The burner block is the piece that carries the burner through the furnace wall into the flame zone, where it sees both high temperature and violent gas flow. Two material families are produced for it, corundum-mullite based and mullite based, both with high strength, good thermal resistance and good performance in burner lining service. The block is designed around the specific burner structure and service condition rather than supplied as a standard item.

Why does a furnace roof need expansion joints, and what goes in them?

A suspended roof expands as it heats and the expansion has to go somewhere, because a rigid roof will crack. Ceramic fibre paper or high-grade polycrystalline microporous board fills the reserved gaps and is crushed as the lining expands, absorbing the destructive volume movement so the rigid refractory is not crushed and spalled. The filler is the sacrificial element in the joint.

How do I choose between plastic refractory and castable for a furnace roof?

Plastic refractory is a semi-wet material that is pressed or extruded into blocks and deformed by hammer impact, so it packs perfectly around irregular geometry and gives excellent installation integrity. It is characterised by good installation property, good thermal shock resistance, low thermal expansion and good thermal insulation, which makes it well suited to roofs and fume pipes. Castable is chosen where cast-in-place geometry is acceptable and faster installation matters.

What does anchor brick have to survive?

Anchor brick resists the load of the suspended lining and the heat of the furnace at the same time, so it must combine high compressive strength with good thermal shock resistance and good abrasion resistance. Anchor spacing is a standard grid, typically 250 to 300 mm centres, and the anchor length has to suit the lining thickness so the weld stays clear of the hot face.

When should I use a light-weight castable or ceramic fibre behind a dense working layer?

Whenever the thermal budget is the constraint rather than the abrasion. The dense grade goes on the hot face and the light-weight grade or ceramic fibre goes behind it as the thermal barrier. That combination lowers shell temperature and heat loss, cuts the thermal shock reaching the hot face, and reduces fuel consumption, without giving up abrasion resistance where it actually matters.

How do I read furnace shell temperature to judge the lining?

Shell surface temperature is the direct indicator of how much heat is escaping through the lining. It is the cheapest continuous health check available. Ladle and cement kiln shells are targeted below 350 °C, and an ultra-high-power electric arc furnace shell below 250 °C. A rising trend at one location usually means the lining in that zone has thinned and the next shutdown will find it.

Refractory Lining Engineering, Installation and Troubleshooting

Questions: 48

Questions in this section
  1. Selection & Technical Data (8)
  2. Lining Design (10)
  3. Installation, Curing & Baking (8)
  4. Failure Diagnosis (9)
  5. Service Life, Maintenance & Repair (8)
  6. Testing, Standards & Procurement (5)

Selection & Technical Data

Q1. How do I choose between shaped brick, castable, gunning mix and dry mass?

Shaped brick gives the fastest erection, tight joints and no firing on site, but it carries the joint count and the mortar. Low-cement castable gives a joint-free lining with the best thermal-shock tolerance and the highest integrity, but it needs curing, drying and a controlled bake. Gunning mix is the only option that repairs a hot face without shutting the furnace, at the cost of rebound losses. Dry mass is for permanent linings and furnace bottoms where water cannot be introduced.

Q2. Which numbers on a refractory technical data sheet actually drive the decision?

Six. Apparent porosity, because every connected pore is a path for slag and gas penetration. Bulk density, because it sets the heat storage and the thermal gradient behind the lining. Cold crushing strength for mechanical integrity. Modulus of rupture, because brick fails in bending long before it fails in compression. Refractoriness under load, because it is the only property that tells you whether the material carries weight at temperature. Permanent linear change, because that is the volume change the expansion joints must absorb.

Q3. How do I select the chemistry grade for a steelmaking slag?

Match the refractory basicity to the slag basicity, and read the FeO content first. FeO is the most aggressive component against MgO-C brick because it dissolves the periclase and oxidises the graphite. A high-FeO, low-MgO slag needs a higher grade, higher carbon content and a tighter protective layer. A higher-MgO slag is far less aggressive and allows a lower grade to be used.

Q4. How much carbon should a MgO-C brick have for a ladle working layer?

It is a direct trade-off. More carbon gives better slag resistance, higher thermal shock resistance and lower porosity; less carbon gives better thermal conductivity and lower cost but loses slag resistance. Ladle working layers typically run at the higher-carbon end with permanent layers lower, and the final grade is selected against the actual slag analysis rather than by rule of thumb.

Q5. When do I need a magnesia-alumina spinel brick instead of MgO-C?

When carbon contamination of the steel is unacceptable, for example clean steel, low-carbon and ultra-low-carbon grades, and stainless applications where carbon pickup is a quality rejection. Spinel brick carries no carbon, has no carbon pick-up risk, and gives up some slag resistance against highly basic slags as the price. It is a specification decision driven by the steel grade, not by cost.

Q6. Which refractories are safe for clean and low-carbon steel production?

The requirement is zero carbon pickup, which removes MgO-C from the working layer. The route is high-temperature carbon-free resin-bonded brick, ultra-low-carbon strong and tough MgO-C brick, pure low-carbon corundum-spinel brick for the bottom blowing impact zone, and carbon-free dry environmentally friendly coating for the tundish, so that both carburisation and hydrogen pick-up are eliminated.

Q7. When do I use a light-weight castable instead of a dense one?

Behind the working layer, always. The working layer takes the abrasion and the dense backing behind it takes the heat. A light-weight or insulating castable behind the hot face allows the total lining thickness to be cut, which lowers shell temperature, reduces thermal shock on the hot face and lowers fuel consumption.

Q8. What is the difference between refractoriness and refractoriness under load?

Refractoriness is the temperature at which the material begins to soften on the pyrometric cone scale, so it is a material identity number rather than a service number. Refractoriness under load is the temperature at which the material fails while carrying a standard mechanical load, so it is the only one of the four that describes load-bearing capability. It normally runs 200 to 300 °C below refractoriness, and selecting on refractoriness alone is a common and expensive mistake.

Lining Design

Q9. How thick should the working lining and the permanent lining be?

The working layer is sized to the wear rate of that zone divided by the acceptable loss per campaign, and it is the thin part. The permanent lining behind it is sized so that a full breach of the working layer does not reach steel within one campaign, and it also carries most of the insulation duty. In a ladle, a working lining of a few tens of millimetres over a much thicker permanent lining is the normal arrangement.

Q10. What expansion joint allowance do I use, and how is it calculated?

Calculate the expected thermal movement of the lining over its free length, divide it by the number of joints you are prepared to install, then add the manufacturing tolerance of the joint filler. For magnesia and magnesia-carbon the movement is significant because of the high thermal expansion of the periclase, so typical practice allows roughly 1.5% to 2% of the free lining length, which works out at roughly 15 to 20 mm of total joint opening per metre of wall height. The final number must come from the supplier's expansion data for the actual brick.

Q11. How far apart should expansion joints be spaced?

Close enough that each joint absorbs its share of the movement, and aligned with the geometry: corners, openings, changes of section and the junction between old and new lining. A common practice for vertical furnace walls is one joint roughly every 1.0 to 1.5 m. Joints must also be staggered between lining courses so that a continuous vertical weakness is not created.

Q12. What goes into the expansion joint, and how thick should it be?

Compressible ceramic fibre paper, or a high-grade polycrystalline microporous board, sized so it fills the gap and can be crushed by the lining as it expands. The filler's job is to absorb the destructive volume change of the brick so the brick itself is not crushed and spalled. The fibre also blocks the gas path through the joint.

Q13. Do silica brick linings need different joint treatment from magnesia?

Yes. Silica has a different expansion behaviour and a lower-temperature transition, so both the joint design and the bake curve through that transition differ from magnesia. Magnesia linings also demand attention during the bake because their expansion is more continuous. Joint allowance must always be taken from the specific material's data rather than from another material's rule.

Q14. What anchor type and spacing do you use?

Heat-resistant stainless steel anchors welded to the casing and buried in the castable, on a grid of roughly 250 to 300 mm centres. Anchor length has to suit the lining thickness so the anchor tip sits inside the lining while the weld stays clear of the hot face. Anchors set the pattern of the cracking that will happen later, so their placement decides whether the lining fails in a contained way or across a whole panel.

Q15. Does brick size affect lining performance?

It affects the joint count, and the joint count governs penetration. Fewer, larger bricks mean fewer mortar joints, less joint area to leak through and faster installation, but they need bigger handling equipment and more careful setting out. The standard stock module in the catalogue is 230 x 114 x 65 mm and most specifications are built around it.

Q16. How thick should the mortar joint be, and why does joint fullness matter?

Thin, typically 1 to 3 mm for alumina brick with mortar, while magnesia and silica are commonly laid dry with a minimum joint. A thick joint is a weak joint: it shrinks, it cracks and it becomes a channel. A full, consistent joint keeps the hot face continuous and stops slag finding a path between the bricks. Mortar refractoriness is normally set slightly below the brick for this reason.

Q17. Why does a brick lining behave differently from a castable lining under the same duty?

A brick lining is many units with many interfaces, and each interface is a potential leak path and a place where stress concentrates. A castable lining is monolithic, so it fails as one body rather than as a set of units, and it has no joints to seal. But it carries its own constraint: it must be cured, dried and baked before service, and that has to be planned into the shutdown.

Q18. How should the working lining be laid out so the hot face stays continuous?

Design the bond so that no continuous vertical or horizontal joint runs through the full lining thickness, stagger the courses, and close out the joints of one course with the middle of the brick in the next. Where the lining changes thickness, use a stepped transition rather than a butt joint, and put the expansion joint where the change occurs rather than carrying it through.

Installation, Curing & Baking

Q19. What is the correct way to mix castable?

Only in a paddle or planetary forced mixer. Manual turning and free-fall drum concrete mixers are strictly prohibited because they entrain air and leave the mix uneven. Add the metered quantity of pure water according to the product data sheet, mix quickly for 3 to 5 minutes until the slurry is uniform, then place and compact by vibration.

Q20. How much water should I add, and what happens if I add too much?

Follow the data sheet. Low-cement castables normally need only 4.5% to 7.5% water addition, and excess water raises porosity, cuts strength and can cause steam spalling during drying. Once the slurry begins to set, no secondary water addition and remixing is allowed, because the strength will plummet permanently.

Q21. How much curing and drying time does a new castable lining need?

After installation and demoulding, the lining is covered with wet sacks or sprayed with curing agent for at least 24 hours of natural curing at normal temperature, so the cement hydration network can form. Drying and baking follow on a strict curve: a slow heating rate of 20 to 30 °C per hour to 200 °C with a long hold to exhaust moisture, then 30 to 50 °C per hour to the process operating temperature.

Q22. What is the standard baking curve, and why are the holds there?

The shape is standard even where the numbers are product-specific: a slow ramp of roughly 20 to 30 °C per hour up to 200 °C, a long hold there to exhaust moisture, then 30 to 50 °C per hour up to the process temperature. The hold exists because free water and crystal water come off at different temperatures, and if that water is driven off too fast the internal steam pressure exceeds the strength of the material and the lining spalls.

Q23. Why does preheating matter so much, and what happens if I rush it?

Newly built linings contain large amounts of free water and crystal water. Forced heating without following the curve vaporises that water rapidly, generates huge internal steam pressure and causes lining explosion and collapse. Preheating also eliminates the structural thermal stress gradient that would otherwise be locked in on the first charge. A detailed furnace drying and preheating curve chart is supplied with each batch of material.

Q24. How do I control the CO and CO2 released on the first heat?

This comes from the decomposition of the binder and from oxidation of carbon in the brick, so the control is in the ramp rate and in the vent path. Bring the furnace up on the specified curve with good extraction and a clear offgas route, and do not let the temperature sit high in the decomposition range without flow. Where carbon loss at the surface would be unacceptable for the steel grade, select a carbon-free or low-carbon grade for that zone instead of trying to manage the offgas.

Q25. How long does a typical ladle overhaul take, and how is it shortened?

Through material upgrades and engineering optimisation, overhaul downtime is compressed heavily. In 200 to 300 ton ladle projects combined with hot-face red-hot gunning solutions, the frequency of full relining is reduced. Local rapid hot repair of the slag line or impact pad takes 6 to 10 hours, and with a fully modular precast block lifting solution the entire cold repair can be cut from several days to within 6 to 12 hours.

Q26. What installation methods do you use for each product family?

Shaped bricks are laid in a staggered bond with special fireclay mortar, with precise expansion joints reserved and steel strips or anchors for fastening. Castables are force-mixed, vibrated after mould filling, wet-cured and baked on curve. Plastics are pneumatically rammed with air picks. Gunning mixes are sprayed at high pressure. Precast blocks are factory customised and lifted and welded on site.

Failure Diagnosis

Q27. What are the failure modes of a lining, and how do I tell them apart?

Three, and they are distinguished by what the wear surface looks like. Thermal-shock spalling shows as flakes and cracks with clean fracture faces, usually concentrated where heat transfer is highest. Slag erosion shows as a smooth, dished, chemically penetrated surface. Mechanical damage shows as localised impact and displacement. Correct diagnosis before changing the material is essential, because each one has a different remedy.

Q28. The slag line of my ladle erodes faster than expected. What do I check?

In order: the slag analysis itself, since FeO content and the MgO/CaO ratio set the aggression; then whether the grade specified for that zone is the grade actually installed; then brick dimensions and joint quality in the slag line zone; then whether expansion joints are correctly placed and sized in that band; then the operating pattern, since long holding times at high temperature and aggressive tapping concentrate attack there.

Q29. Does steel temperature affect the slag attack rate?

Yes, strongly, and not linearly. Superheat lowers slag viscosity, and lower viscosity raises both penetration and wash-out rates sharply. As a working rule, every additional 50 °C of tapping temperature can roughly double the penetration rate within a typical range. This is why practices that reduce turndown and stabilise tapping temperature outperform brick upgrades alone, and why the same grade can perform well in one plant and fail in another.

Q30. Why is my castable cracking after the 110 °C drying stage?

Three usual causes: too much water in the mix, which raises porosity and shrinkage; a drying ramp or hold not matched to the section thickness, so steam pressure exceeded the green strength; or a curing failure where the surface dried before hydration completed. Check the mix record against the data sheet, and re-check the curve against the actual thickness rather than a generic one.

Q31. Why is my gunning rebound rate so high?

Rebound is material lost as overspray rather than sticking. The usual causes are too much water in the mix, a worn or wrong nozzle, too great a spraying distance, and spraying onto a surface that is too cold or too dirty to accept the material. High rebound wastes product and slows the repair, and the same conditions also produce a weak, poorly bonded repair that will spall out again.

Q32. What does the shell temperature tell me, and what are the target limits?

It is the most direct and cheapest indicator of how much heat is escaping through the lining, and therefore of how much life is left. The optimisation targets are a ladle shell controlled below 350 °C, a cement kiln shell below 350 °C, and an ultra-high-power electric arc furnace shell below 250 °C. A rising trend on one spot is the early warning that a zone has thinned.

Q33. How do I determine the actual lining wear rate?

Three methods, used together. Precise residual thickness physical measurement during overhaul shutdown. Chemical penetration phase analysis and microscopic scanning of sampled discarded residual bricks. And a review of the operating data against the results: maximum temperature, thermal cycling periods and abnormal slag chemistry. The findings feed back into the next formulation revision.

Q34. What is thermal shock stability, and how is it measured?

It measures the ability to resist internal thermal stress without cracking or surface spalling under severe rapid temperature change. In the industry it is calibrated by the number of destructive cycles of rapid water quenching or cold air blowing after heating in a 1,100 °C high-temperature furnace. It is a comparative index and only meaningful when the test condition is stated.

Q35. What is creep, and why does it decide checker brick selection?

Creep refers to the slow and irreversible plastic deformation under the dual action of constant high temperature and long-term static load. The bottom of a hot blast stove checker column, which can be tens of metres of brick above it, bears enormous weight. If the material creeps, the lower courses deform, the gas passages close and the whole regenerator is affected.

Service Life, Maintenance & Repair

Q36. How do I extend ladle campaign life?

Three levers, in order of impact. First, locate the wear with Solidworks 3D thermal modelling and grade the zones separately instead of using one grade everywhere. Second, use the matching brick type in each zone, with the highest grade where the slag line actually is. Third, maintain with red-hot gunning every 5 to 10 heats. Combined, this achieves a 30% reduction in refractory cost and downtime alongside an extension of overall ladle service life by up to 30%.

Q37. What hot repair solutions are available?

Full life-cycle life extension escort for high-temperature equipment. High-temperature fast-setting castables for emergency repair of sudden furnace penetration, and high-pressure gunning mix solutions for regularly restoring slag line thickness within planned schedules. Standard spare parts in stock are committed to extremely fast shipment within 48 hours.

Q38. What is the difference between gunning and shotcreting?

Gunning mostly uses semi-dry material, driven by high-pressure air onto the red-hot old furnace lining surface, sintering instantly, and is used for thin-layer coverage and emergency hot repair. Shotcreting pumps a wet slurry with accelerators, has extremely low rebound, and can spray extremely thick permanent structural layers in one pass, often for new large furnace chambers or an overall cold overhaul.

Q39. What is the role of ceramic fibre in the expansion joint?

When the furnace temperature rises the bricks expand violently and squeeze each other. The soft ceramic fibre is compressed, and in doing so it absorbs the destructive volume expansion that would otherwise crush and spall the rigid brick. It is the sacrificial element in the joint, and using a filler that is too stiff or the wrong thickness removes that protection entirely.

Q40. Why does the slag line zone fail faster than the rest of the wall?

It sits at the three-phase boundary of gas, slag and liquid in vessels such as ladles and converters, so it takes the highest temperature, the most severe chemical corrosion and the physical wash simultaneously. It is the short-board area that determines the service life of the entire vessel.

Q41. How is 3D CFD simulation used in material selection?

Before the lining is designed, combustion air, combustion air and high-temperature flue gas trajectories are simulated so combustion dead corners are eliminated and heat distribution is made uniform. The lining is then fundamentally protected from biased flow erosion. In hot blast stoves and nonferrous smelting this has changed where material is placed and, as a result, how long the lining lasts.

Q42. How does Solidworks 3D thermal modelling help me choose the lining?

For complex steelmaking vessels, Solidworks 3D software is used for solid modelling analysis of the ladle working lining, slag line, sidewall and bottom blowing impact zone. In actual 200 to 300 ton ladle cases the modelling identified the key hot spots with the most severe lining wear, and comparing three different refractory configuration options helped reduce refractory cost by 30% and shutdown overhaul time by 30%.

Q43. What is the 100% factory pre-assembly process, and how does it help me?

For composite assemblies such as blast furnace tuyere combined bricks, a platform is built in the workshop to the actual 1:1 dimensions and the finished bricks are completely simulated in assembly. Every brick is checked against the engineering drawing and the reserved gaps, and after a confirmed fit the assembly is spray-coded and packed, ensuring truly zero fit problems at the construction site.

Testing, Standards & Procurement

Q44. What quality tests are run on every batch?

The strictest multi-dimensional laboratory inspection: XRF spectral analysis of the full chemical composition; bulk density and apparent porosity measurement; heavy-duty press measurement of cold crushing strength and modulus of rupture; and verification of refractoriness, refractoriness under load, thermal shock cracking cycles, and high-temperature static and dynamic slag corrosion resistance in high-temperature electric furnaces.

Q45. Which international standards do your products correspond to?

The design and manufacturing system is compatible with mainstream global specifications. The ISO 9001 quality management system audit is fully passed, and physical and chemical indicator measurement can strictly correspond to US ASTM standards, Chinese GB/T mandatory and recommended national standards, or ISO international refractory implementation standards according to customer requirements.

Q46. How should I qualify a new supplier before placing a bulk order?

Run it in stages. Audit the plant and the quality system first. Then verify that the supplier's certificate is issued by an accredited laboratory with the correct standard stated, not merely self-declared. Then run a controlled trial installation in one zone, compare measured properties against the data sheet, and check that the batch code on the certificate physically matches the delivery. Only then release the main order.

Q47. How do I calculate my annual refractory consumption?

Build it from two streams. Planned relining consumption is the number of units to be lined times the lining area per unit times the lining thickness times the installed density, plus a waste and damage factor. Repair consumption is the perimeter times the worn area times the material applied per repair event times the number of events per year, plus gunning material used for touch-up. Then reconcile the calculated figure against actual purchase and site issue records.

Q48. How should refractory cement, binders and unshaped materials be stored?

Strict storage environment requirements. Dry bagged moisture-proof castables are stored indoors in a dry, ventilated place for 6 to 12 months. Plastics containing liquid binders have a shorter shelf life, usually 3 to 6 months. Precast blocks that have been thoroughly high-temperature baked and shaped have almost no shelf life limit as long as they are kept dry.